'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Overview_of_chemicals click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Overview_of_chemicals click here]'''
 
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''
 
'''All links to Labmanager requires login.'''
 
'''All measurements on this page has been made by Nanolab staff.'''  


=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=
=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=
Descreption: On this page you can have an overveiw of the standardt Chimicals we have in the Cleenroom, as well as link to Kemibrug for those chemicals. you will also be able to see if there is any change in the chemicals we have or something else about them in the commets.


{| border="2" cellspacing="0" cellpadding="10"  
{| border="2" cellspacing="0" cellpadding="10"  
Line 18: Line 25:
|-
|-
!style="background:silver; color:black;" align="left"|Ammoniumhydroxyd
!style="background:silver; color:black;" align="left"|Ammoniumhydroxyd
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier?casnr=1336-21-6&pnr=&KBAOnly=false&SearchInNotes=false&NormalSearchKemikalier=true&NormalSearchKemikalier=false&WildCardSearchKemikalier=false&ExactSearchKemikalier=false&inklNoter=false&selectedLangtidsvirkning= Cas Nr. 1336-21-6]
1336-21-6  
!style="background:LightGrey; color:black;"|28%
!style="background:LightGrey; color:black;"|28%
!style="background:LightGrey; color:black;"|VLSI
!style="background:LightGrey; color:black;"|VLSI
Line 25: Line 31:
|-
|-
!style="background:silver; color:black;" align="left"|Ammoniumperoxodisulfat
!style="background:silver; color:black;" align="left"|Ammoniumperoxodisulfat
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESUlKRUpFRVRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. 7727-54-0]
7727-54-0
!style="background:LightGrey; color:black;"|98%-99,1%
!style="background:LightGrey; color:black;"|98%-99,1%
!style="background:LightGrey; color:black;"|Analyse
!style="background:LightGrey; color:black;"|Analyse
Line 32: Line 37:
|-
|-
!style="background:silver; color:black;" align="left"|Anisole Anhydrous
!style="background:silver; color:black;" align="left"|Anisole Anhydrous
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESU1NTkVKVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K Cas Nr. 100-66-3]
100-66-3
!style="background:LightGrey; color:black;"|99,7%
!style="background:LightGrey; color:black;"|99,7%
!style="background:LightGrey; color:black;"|GPR
!style="background:LightGrey; color:black;"|GPR
Line 39: Line 43:
|-
|-
!style="background:silver; color:black;" align="left"|AR-600-546 Developer
!style="background:silver; color:black;" align="left"|AR-600-546 Developer
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhERkZLSEtGS1RkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.
!style="background:LightGrey; color:black;"|not specified
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specified
!style="background:LightGrey; color:black;"|not specific
!style="background:WhiteSmoke; color:black"|Comment
!style="background:WhiteSmoke; color:black"|Comment
|-
|-
!style="background:silver; color:black;" align="left"|AR-600-71 Remover
!style="background:silver; color:black;" align="left"|AR-600-71 Remover
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhERkZLRkxFRlRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific  
!style="background:LightGrey; color:black;"|not specific  
Line 53: Line 55:
|-
|-
!style="background:silver; color:black;" align="left"|AR-6200.09 E-beam resist
!style="background:silver; color:black;" align="left"|AR-6200.09 E-beam resist
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhERkZLR0xMSVRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.  
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific  
!style="background:LightGrey; color:black;"|not specific  
Line 60: Line 61:
|-
|-
!style="background:silver; color:black;" align="left"|AZ 351B Developer
!style="background:silver; color:black;" align="left"|AZ 351B Developer
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhES01NTUdMRVRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.  
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific  
!style="background:LightGrey; color:black;"|not specific  
Line 67: Line 67:
|-
|-
!style="background:silver; color:black;" align="left"|AZ 4562 Photoresist
!style="background:silver; color:black;" align="left"|AZ 4562 Photoresist
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETEtKSEVKSFRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.  
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
Line 74: Line 73:
|-
|-
!style="background:silver; color:black;" align="left"|AZ 5214E Photoresist
!style="background:silver; color:black;" align="left"|AZ 5214E Photoresist
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETEdKTEdJSFRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.  
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific  
!style="background:LightGrey; color:black;"|not specific  
Line 81: Line 79:
|-
|-
!style="background:silver; color:black;" align="left"|AZ 726MIF developer
!style="background:silver; color:black;" align="left"|AZ 726MIF developer
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETkVFTUVGR1RkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific  
!style="background:LightGrey; color:black;"|not specific  
Line 88: Line 85:
|-
|-
!style="background:silver; color:black;" align="left"|AZ 726MIF developer (Tromle)
!style="background:silver; color:black;" align="left"|AZ 726MIF developer (Tromle)
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETkVFTUVGR1RkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
Line 95: Line 91:
|-
|-
!style="background:silver; color:black;" align="left"|AZ MiR 701 (29CPS) Photoresist
!style="background:silver; color:black;" align="left"|AZ MiR 701 (29CPS) Photoresist
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhERkVGTU5NSFRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. No nr.]
no nr.
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific  
!style="background:LightGrey; color:black;"|not specific  
Line 102: Line 97:
|-
|-
!style="background:silver; color:black;" align="left"|AZ nLOF 2020 Photoresist
!style="background:silver; color:black;" align="left"|AZ nLOF 2020 Photoresist
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETEtGS0ZNSVRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific  
!style="background:LightGrey; color:black;"|not specific  
Line 109: Line 103:
|-
|-
!style="background:silver; color:black;" align="left"|Boric Acid powder
!style="background:silver; color:black;" align="left"|Boric Acid powder
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETUZGS0pJR1RkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. 10043-35-3]
10043-35-3
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|Analytic
!style="background:LightGrey; color:black;"|Analytic
Line 116: Line 109:
|-
|-
!style="background:silver; color:black;" align="left"|Chrome etch 18
!style="background:silver; color:black;" align="left"|Chrome etch 18
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhES0hHR0pMS1RkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.  
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific  
!style="background:LightGrey; color:black;"|not specific  
Line 123: Line 115:
|-
|-
!style="background:silver; color:black;" align="left"|Developer MIBK Methylisobutylketon 4L
!style="background:silver; color:black;" align="left"|Developer MIBK Methylisobutylketon 4L
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETE5FSkVMS1RkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. 108-10-1]
108-10-1
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|VLSI
!style="background:LightGrey; color:black;"|VLSI
Line 130: Line 121:
|-
|-
!style="background:silver; color:black;" align="left"|DUV42S-6,4 L ultra nowpak W/Closure lid
!style="background:silver; color:black;" align="left"|DUV42S-6,4 L ultra nowpak W/Closure lid
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhERkdNR0tITVRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.  
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|Aicello
!style="background:LightGrey; color:black;"|Aicello
Line 137: Line 127:
|-
|-
!style="background:silver; color:black;" align="left"|Ethanol
!style="background:silver; color:black;" align="left"|Ethanol
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETUpFRklGS1RkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. 64-17-5]
64-17-5  
!style="background:LightGrey; color:black;"|99,9%-100%
!style="background:LightGrey; color:black;"|99,9%-100%
!style="background:LightGrey; color:black;"|VLSI  
!style="background:LightGrey; color:black;"|VLSI  
Line 144: Line 133:
|-
|-
!style="background:silver; color:black;" align="left"|Hydrofluoric acid buffer (BHF/BOE)
!style="background:silver; color:black;" align="left"|Hydrofluoric acid buffer (BHF/BOE)
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETUdJSUpNS1RkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.
!style="background:LightGrey; color:black;"|12,5%
!style="background:LightGrey; color:black;"|12,5%
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
Line 151: Line 139:
|-
|-
!style="background:silver; color:black;" align="left"|Hydrofluoric acid buffer (BHF/BOE W/wetting agent)
!style="background:silver; color:black;" align="left"|Hydrofluoric acid buffer (BHF/BOE W/wetting agent)
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETUZKS01LSlRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.
!style="background:LightGrey; color:black;"|12,5%
!style="background:LightGrey; color:black;"|12,5%
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
Line 158: Line 145:
|-
|-
!style="background:silver; color:black;" align="left"|Hexamethyldisilasan
!style="background:silver; color:black;" align="left"|Hexamethyldisilasan
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhER0VFRkxJVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K Cas Nr. 999-97-3]
999-97-3
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
Line 165: Line 151:
|-
|-
!style="background:silver; color:black" align="left" valign="top" rowspan="4"|HYDROFLUORIC ACID (HF)
!style="background:silver; color:black" align="left" valign="top" rowspan="4"|HYDROFLUORIC ACID (HF)
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETUhLSkpITVRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.
|style="background:LightGrey; color:black"|1%
|style="background:LightGrey; color:black"|1%
!style="background:LightGrey; color:black;"|VLSI
!style="background:LightGrey; color:black;"|VLSI
|style="background:WhiteSmoke; color:black"|Comment
|style="background:WhiteSmoke; color:black"|Comment
|-
|-
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETUhLSkhLTlRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. No nr.]
no nr.
|style="background:LightGrey; color:black"|10%
|style="background:LightGrey; color:black"|10%
!style="background:LightGrey; color:black;"|VLSI
!style="background:LightGrey; color:black;"|VLSI
|style="background:WhiteSmoke; color:black"|Comment
|style="background:WhiteSmoke; color:black"|Will be removed ones we no longer have any in storage
|-  
|-  
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETUhLSktOTFRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.
|style="background:LightGrey; color:black"|40%
|style="background:LightGrey; color:black"|40%
!style="background:LightGrey; color:black;"|EMSURE® ISO for analysis
!style="background:LightGrey; color:black;"|EMSURE® ISO for analysis
|style="background:WhiteSmoke; color:black"|Comment
|style="background:WhiteSmoke; color:black"|Comment
|-
|-
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhES0pJTEtJR1RkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.
|style="background:LightGrey; color:black"|50%
|style="background:LightGrey; color:black"|50%
!style="background:LightGrey; color:black;"|VLSI
!style="background:LightGrey; color:black;"|VLSI
Line 190: Line 172:
|-
|-
!style="background:silver; color:black;" align="left"|Hydrochloric acid
!style="background:silver; color:black;" align="left"|Hydrochloric acid
!style="background:LightGrey; color:black;"|Cas Nr. 7647-01-0
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETElITUpITlRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. 7647-01-0]
!style="background:LightGrey; color:black;"|37%
!style="background:LightGrey; color:black;"|37%
!style="background:LightGrey; color:black;"|VLSI
!style="background:LightGrey; color:black;"|VLSI
Line 196: Line 178:
|-
|-
!style="background:silver; color:black;" align="left"|Hydrogenperoxid
!style="background:silver; color:black;" align="left"|Hydrogenperoxid
!style="background:LightGrey; color:black;"|Cas Nr. 7722-84-1
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESUlKRUVISVRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. 7722-84-1]
!style="background:LightGrey; color:black;"|31%
!style="background:LightGrey; color:black;"|31%
!style="background:LightGrey; color:black;"|VLSI
!style="background:LightGrey; color:black;"|VLSI
Line 202: Line 184:
|-
|-
!style="background:silver; color:black;" align="left"|KRF m230Y 6cP Gal
!style="background:silver; color:black;" align="left"|KRF m230Y 6cP Gal
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESkpGSk1GSVRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
Line 209: Line 190:
|-
|-
!style="background:silver; color:black;" align="left"|KRF M35G 27cP Gal
!style="background:silver; color:black;" align="left"|KRF M35G 27cP Gal
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESkpGSklKRlRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
Line 216: Line 196:
|-
|-
!style="background:silver; color:black;" align="left"|Microposit Remover 1165  
!style="background:silver; color:black;" align="left"|Microposit Remover 1165  
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhES0VOSUpFVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K Cas Nr. no nr.]
no nr.
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|Grade
!style="background:LightGrey; color:black;"|Grade
Line 223: Line 202:
|-
|-
!style="background:silver; color:black;" align="left"|Nitric acid  
!style="background:silver; color:black;" align="left"|Nitric acid  
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETEpITkVGTFRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. 231-714-2]
231-714-2
!style="background:LightGrey; color:black;"|69%
!style="background:LightGrey; color:black;"|69%
!style="background:LightGrey; color:black;"|VLSI
!style="background:LightGrey; color:black;"|VLSI
Line 230: Line 208:
|-
|-
!style="background:silver; color:black;" align="left"|Ortho-Phosphoric acid
!style="background:silver; color:black;" align="left"|Ortho-Phosphoric acid
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETElMTEdOS1RkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. 7664-38-2]
7664-38-2
!style="background:LightGrey; color:black;"|85%
!style="background:LightGrey; color:black;"|85%
!style="background:LightGrey; color:black;"|VLSI
!style="background:LightGrey; color:black;"|VLSI
Line 237: Line 214:
|-
|-
!style="background:silver; color:black;" align="left"|Potassium hydroxide solution
!style="background:silver; color:black;" align="left"|Potassium hydroxide solution
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETE1IS0xIRVRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. 1310-58-3]
1310-58-3
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|Selectipur
!style="background:LightGrey; color:black;"|Selectipur
!style="background:WhiteSmoke; color:black"|Comment
!style="background:WhiteSmoke; color:black"|Comment
|-
|-
!style="background:silver; color:black;" align="left"|Propanol
!style="background:silver; color:black;" align="left"|Isoropanol
!style="background:LightGrey; color:black;"|Cas Nr.  
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETEhITUlHRlRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. 67-63-0]
67-63-0
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|VLSi
!style="background:LightGrey; color:black;"|VLSi
Line 251: Line 226:
|-
|-
!style="background:silver; color:black;" align="left"|SU-8 2005
!style="background:silver; color:black;" align="left"|SU-8 2005
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhES0lFRUVJVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K Cas Nr. no .nr]
no .nr
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
Line 258: Line 232:
|-
|-
!style="background:silver; color:black;" align="left"|SU-8 2035
!style="background:silver; color:black;" align="left"|SU-8 2035
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhES0lFRUVJVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K Cas Nr. no .nr]
no nr.
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
Line 265: Line 238:
|-
|-
!style="background:silver; color:black;" align="left"|SU-8 2075
!style="background:silver; color:black;" align="left"|SU-8 2075
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhES0lFRUVJVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K Cas Nr. no .nr]
no nr.
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
Line 272: Line 244:
|-
|-
!style="background:silver; color:black;" align="left"|SU-8 Developer (Mr-dev 600)
!style="background:silver; color:black;" align="left"|SU-8 Developer (Mr-dev 600)
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETkdITklFVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K Cas Nr. no nr.]
no nr.
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
Line 279: Line 250:
|-
|-
!style="background:silver; color:black;" align="left"|SU-8 Thinner
!style="background:silver; color:black;" align="left"|SU-8 Thinner
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhES0dLRktGVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K Cas Nr. no nr.]
no nr.
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
Line 286: Line 256:
|-
|-
!style="background:silver; color:black;" align="left"|Sulfamic acid  
!style="background:silver; color:black;" align="left"|Sulfamic acid  
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESklISUVLS1RkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. 5329-14-6]
5329-14-6
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|Alkamlimetry
!style="background:LightGrey; color:black;"|Alkamlimetry
Line 293: Line 262:
|-
|-
!style="background:silver; color:black;" align="left"|Sulfuric acid  
!style="background:silver; color:black;" align="left"|Sulfuric acid  
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETElMTk1GTFRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. 7664-93-9]
7664-93-9
!style="background:LightGrey; color:black;"|95%-97%
!style="background:LightGrey; color:black;"|95%-97%
!style="background:LightGrey; color:black;"|VLSI
!style="background:LightGrey; color:black;"|VLSI
Line 300: Line 268:
|-
|-
!style="background:silver; color:black;" align="left"|TI spray  
!style="background:silver; color:black;" align="left"|TI spray  
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETUlHSE1NTFRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. no nr.]
no nr.
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
Line 307: Line 274:
|-
|-
!style="background:silver; color:black;" align="left"|ZED N50
!style="background:silver; color:black;" align="left"|ZED N50
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESkpOTUlMVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K Cas Nr. no nr.]
no nr.
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
Line 314: Line 280:
|-
|-
!style="background:silver; color:black;" align="left"|Triton x-100
!style="background:silver; color:black;" align="left"|Triton x-100
!style="background:LightGrey; color:black;"|Cas Nr.
!style="background:LightGrey; color:black;"|[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhETEdORUlJRlRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K Cas Nr. 9002-93-1]
9002-93-1
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific
!style="background:LightGrey; color:black;"|not specific

Latest revision as of 11:21, 27 February 2023

Feedback to this page: click here

Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.

All links to Labmanager requires login.

All measurements on this page has been made by Nanolab staff.

THIS PAGE IS UNDER CONSTRUCTION

Descreption: On this page you can have an overveiw of the standardt Chimicals we have in the Cleenroom, as well as link to Kemibrug for those chemicals. you will also be able to see if there is any change in the chemicals we have or something else about them in the commets.

Chemical Cas Nr. Concentration Grade Comment
Acetone Cas Nr. 67-64-1 99,8%-100% VLSi
Ammoniumhydroxyd Cas Nr. 1336-21-6 28% VLSI Comment
Ammoniumperoxodisulfat Cas Nr. 7727-54-0 98%-99,1% Analyse Comment
Anisole Anhydrous Cas Nr. 100-66-3 99,7% GPR Comment
AR-600-546 Developer Cas Nr. no nr. not specified not specified Comment
AR-600-71 Remover Cas Nr. no nr. not specific not specific Comment
AR-6200.09 E-beam resist Cas Nr. no nr. not specific not specific Comment
AZ 351B Developer Cas Nr. no nr. not specific not specific Comment
AZ 4562 Photoresist Cas Nr. no nr. not specific not specific Comment
AZ 5214E Photoresist Cas Nr. no nr. not specific not specific Comment
AZ 726MIF developer Cas Nr. no nr. not specific not specific Comment
AZ 726MIF developer (Tromle) Cas Nr. no nr. not specific not specific Comment
AZ MiR 701 (29CPS) Photoresist Cas Nr. No nr. not specific not specific Comment
AZ nLOF 2020 Photoresist Cas Nr. no nr. not specific not specific Comment
Boric Acid powder Cas Nr. 10043-35-3 not specific Analytic Comment
Chrome etch 18 Cas Nr. no nr. not specific not specific Comment
Developer MIBK Methylisobutylketon 4L Cas Nr. 108-10-1 not specific VLSI Comment
DUV42S-6,4 L ultra nowpak W/Closure lid Cas Nr. no nr. not specific Aicello Comment
Ethanol Cas Nr. 64-17-5 99,9%-100% VLSI Comment
Hydrofluoric acid buffer (BHF/BOE) Cas Nr. no nr. 12,5% not specific Comment
Hydrofluoric acid buffer (BHF/BOE W/wetting agent) Cas Nr. no nr. 12,5% not specific Comment
Hexamethyldisilasan Cas Nr. 999-97-3 not specific not specific Comment
HYDROFLUORIC ACID (HF) Cas Nr. no nr. 1% VLSI Comment
Cas Nr. No nr. 10% VLSI Will be removed ones we no longer have any in storage
Cas Nr. no nr. 40% EMSURE® ISO for analysis Comment
Cas Nr. no nr. 50% VLSI Comment
Hydrochloric acid Cas Nr. 7647-01-0 37% VLSI Comment
Hydrogenperoxid Cas Nr. 7722-84-1 31% VLSI Comment
KRF m230Y 6cP Gal Cas Nr. no nr. not specific not specific Comment
KRF M35G 27cP Gal Cas Nr. no nr. not specific not specific Comment
Microposit Remover 1165 Cas Nr. no nr. not specific Grade Comment
Nitric acid Cas Nr. 231-714-2 69% VLSI Comment
Ortho-Phosphoric acid Cas Nr. 7664-38-2 85% VLSI Comment
Potassium hydroxide solution Cas Nr. 1310-58-3 not specific Selectipur Comment
Isoropanol Cas Nr. 67-63-0 not specific VLSi Comment
SU-8 2005 Cas Nr. no .nr not specific not specific Comment
SU-8 2035 Cas Nr. no .nr not specific not specific Comment
SU-8 2075 Cas Nr. no .nr not specific not specific Comment
SU-8 Developer (Mr-dev 600) Cas Nr. no nr. not specific not specific Comment
SU-8 Thinner Cas Nr. no nr. not specific not specific Comment
Sulfamic acid Cas Nr. 5329-14-6 not specific Alkamlimetry Comment
Sulfuric acid Cas Nr. 7664-93-9 95%-97% VLSI Comment
TI spray Cas Nr. no nr. not specific not specific Comment
ZED N50 Cas Nr. no nr. not specific not specific Comment
Triton x-100 Cas Nr. 9002-93-1 not specific not specific Comment