'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Chromium/Sputtering_of_Cr_in_Sputter_System_(Lesker) click here]'''
<i>This page is written by <b>Evgeniy Shkondin @DTU Nanolab</b> if nothing else is stated. <br>
<i>This page is written by <b>Evgeniy Shkondin @DTU Nanolab</b> if nothing else is stated. <br>
All images and photos on this page belongs to <b>DTU Nanolab</b>.<br>
All images and photos on this page belongs to <b>DTU Nanolab</b>.<br>

Latest revision as of 20:47, 18 February 2023

Feedback to this page: click here

This page is written by Evgeniy Shkondin @DTU Nanolab if nothing else is stated.
All images and photos on this page belongs to DTU Nanolab.
The fabrication and characterization described below were conducted in 2021-2022 by Evgeniy Shkondin.


Cr Sputtering

This page presents the results of Cr deposition using DC sputtering in Sputter-System Lesker, now commonly known as "Old Lesker". The deposition target is Cr. Source #2 (DC) was used.

The fabrication and characterization described below were conducted in 2021 by Evgeniy Shkondin, DTU Nanolab. The prepared samples were investigated by the X-ray Reflectivity method. The focus of the study was the deposition conditions.


The process recipe in a Sputter-System (Lesker) is following:


  • Deposition type: DC
  • Power: 220 W.
  • Pressure: 3 mTorr
  • Gas: Ar
  • Deposition time: 360
  • Temperature: 20°C (no heating)
  • Measured DC bias: 360V


  • Deposition Rate: 0.148 nm/s



XRR-measurement

Layer parameter list
Layer name Thickness (nm) Density (g/cm3) Rougness (nm) Delta Beta
Moisture 1.73 0.99 0.00 3.0119e-6 6.9942e-8
Cr2O3 4.36 2.96 0.00 8.9602e-6 6.2352e-7
Cr

48.99

6.19 2.93 1.8194e-5 1.8712e-6
SiO2 (native oxide) 2.34 3.02 1.92 9.8053e-6 1.2778e-7
Si (wafer) 2.328 0.00 7.5795e-6 1.7601e-7