Specific Process Knowledge/Etch/III-V ICP/GaAs-AlGaAs: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
Bghe (talk | contribs)
No edit summary
 
(One intermediate revision by the same user not shown)
Line 2: Line 2:
   
   
===GaAs/AlGaAs etching using III-V ICP===
===GaAs/AlGaAs etching using III-V ICP===
'''''Work done by DTU Photonics before 2011'''''
'''''Recipes developed and/or tested by DTU Photonics internal before 2011'''''


{| border="1" cellspacing="2" cellpadding="3"  
{| border="1" cellspacing="2" cellpadding="3"  
Line 135: Line 135:


{| border="1" cellspacing="2" cellpadding="3"  
{| border="1" cellspacing="2" cellpadding="3"  
![[image:ICP_BCL3_result.jpg|300x300px|thumb|left|Result of GaAs etching with BCl<sub>3</sub>. Qijiang Ran, DTU Photonics, 2011. ]]
![[image:ICP_BCL3_result.jpg|300x300px|thumb|left|Result of GaAs etching with BCl<sub>3</sub>. Done by: Qijiang Ran, DTU Photonics, 2011. ]]
|-
|-
|}
|}

Latest revision as of 09:41, 10 February 2023

Feedback to this page: click here

GaAs/AlGaAs etching using III-V ICP

Recipes developed and/or tested by DTU Photonics internal before 2011

Recipe GaAs Etch
Cl2 flow 4 sccm
Ar flow 12 sccm
Platen power 80 W
Coil power 700 W
Pressure 6 mTorr
Platen chiller temperature 20 oC


Results (GaAs Etch)
GaAs etch rate >500 nm/min
Sidewall angle ~ 85-90 o
Selectivity (GaAs:Si3N4, GaAs:AlInP) 10:1, 5:1


Recipe GaAs_AlGaAs Etch
Cl2 flow 20 sccm
N2 flow 50 sccm
Platen power 100 W
Coil power 600 W
Pressure 2 mTorr
Platen chiller temperature 20 oC


Results (GaAs_AlGaAs Etch)
AlGaAs etch rate >1000 nm/min
Sidewall angle ~ 90 o
Selectivity (GaAs:SiO2) 30:1


Recipe GaAs_AlGaAs Etch_BCl3
Cl2 flow 10 sccm
BCl3 flow 10 sccm
Ar flow 10 sccm
N2 flow 4 sccm
Platen power 50 W
Coil power 500 W
Pressure 1 mTorr
Platen chiller temperature 20 oC


Results (GaAs_AlGaAs Etch_BCl3)
GaAs etch rate >750 nm/min
Sidewall angle 85-90 o
Selectivity (GaAs:Si3N4, GaAs:AlInP) 10:1
Result of GaAs etching with BCl3. Done by: Qijiang Ran, DTU Photonics, 2011.