Specific Process Knowledge/Etch/III-V ICP/GaAs-AlGaAs: Difference between revisions
No edit summary |
No edit summary |
||
(5 intermediate revisions by the same user not shown) | |||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/III-V_ICP/GaAs-AlGaAs click here]''' | ||
===GaAs/AlGaAs etching=== | ===GaAs/AlGaAs etching using III-V ICP=== | ||
'''''Recipes developed and/or tested by DTU Photonics internal before 2011''''' | |||
{| border="1" cellspacing="2" cellpadding="3" | {| border="1" cellspacing="2" cellpadding="3" | ||
Line 134: | Line 135: | ||
{| border="1" cellspacing="2" cellpadding="3" | {| border="1" cellspacing="2" cellpadding="3" | ||
![[image:ICP_BCL3_result.jpg|300x300px|thumb|left|Result of GaAs etching with BCl<sub>3</sub>. Qijiang Ran, DTU Photonics, 2011. ]] | ![[image:ICP_BCL3_result.jpg|300x300px|thumb|left|Result of GaAs etching with BCl<sub>3</sub>. Done by: Qijiang Ran, DTU Photonics, 2011. ]] | ||
|- | |- | ||
|} | |} |
Latest revision as of 09:41, 10 February 2023
Feedback to this page: click here
GaAs/AlGaAs etching using III-V ICP
Recipes developed and/or tested by DTU Photonics internal before 2011
Recipe | GaAs Etch |
Cl2 flow | 4 sccm |
Ar flow | 12 sccm |
Platen power | 80 W |
Coil power | 700 W |
Pressure | 6 mTorr |
Platen chiller temperature | 20 oC |
Results (GaAs Etch) | |
GaAs etch rate | >500 nm/min |
Sidewall angle | ~ 85-90 o |
Selectivity (GaAs:Si3N4, GaAs:AlInP) | 10:1, 5:1 |
Recipe | GaAs_AlGaAs Etch |
Cl2 flow | 20 sccm |
N2 flow | 50 sccm |
Platen power | 100 W |
Coil power | 600 W |
Pressure | 2 mTorr |
Platen chiller temperature | 20 oC |
Results (GaAs_AlGaAs Etch) | |
AlGaAs etch rate | >1000 nm/min |
Sidewall angle | ~ 90 o |
Selectivity (GaAs:SiO2) | 30:1 |
Recipe | GaAs_AlGaAs Etch_BCl3 |
Cl2 flow | 10 sccm |
BCl3 flow | 10 sccm |
Ar flow | 10 sccm |
N2 flow | 4 sccm |
Platen power | 50 W |
Coil power | 500 W |
Pressure | 1 mTorr |
Platen chiller temperature | 20 oC |
Results (GaAs_AlGaAs Etch_BCl3) | |
GaAs etch rate | >750 nm/min |
Sidewall angle | 85-90 o |
Selectivity (GaAs:Si3N4, GaAs:AlInP) | 10:1 |