==Barc etch with O2== | ==Barc etch with O2== | ||
'' | {{CC-bghe2}}, ''June 2020'' | ||
===Sample=== | ===Sample=== | ||
*6" Si | *6" Si |
Latest revision as of 11:23, 3 February 2023
Barc etch with O2
Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab, June 2020
Sample
- 6" Si
- 2µm SiO2 from C1
- 90nm barc
- 907 nm UVN 2030-0,5
- Reticle: Pegreticle
- Dose: 200 J/m2
Pegasus 4 settings
- Recipe: Barc O2
- With 30 mm spacers
SEM images after barc etching
-
50% load, 4000 nm pitch, barc has been etched with a little undercut
-
50% load, 2000 nm pitch, barc has been etched with a little undercut
-
75% load, 1600 nm pitch, barc has been etched with a little undercut
-
50% load, 400 nm pitch, barc has been etched with a little undercut expect where the lines have collided
-
50% load, 1300 nm pitch
-
50% load, 800 nm pitch