Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using AOE/Standard recipe with resist mask: Difference between revisions

From LabAdviser
Jump to navigation Jump to search
No edit summary
 
(11 intermediate revisions by the same user not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide/SiO2_etch_using_AOE/Standard_recipe_with_resist_mask  click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide/SiO2_etch_using_AOE/Standard_recipe_with_resist_mask  click here]'''  
{{CC-bghe1}}


=The standard recipe=
=The standard recipe=
Line 43: Line 45:
|
|
*'''~230nm/min (5% etch load)''' -  etch load dependency [[/AOE SiO2 etch load dependency|'''see here''']]
*'''~230nm/min (5% etch load)''' -  etch load dependency [[/AOE SiO2 etch load dependency|'''see here''']]
*~200 nm/min (100% etch load) ''fall 2016 by Martin Lind Ommen @nanotech'' [http://process2share.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_SiO2 '''see here''']
*~200 nm/min (100% etch load) ''fall 2016 by Martin Lind Ommen @nanotech'' [[Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide#Dry_etch_with_Hard_mask|'''see here''']]
|-
|-
|TEOS oxide (5% load)
|TEOS oxide (5% load)
|'''233nm/min ±0.7%''' - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 ''by LN/BGE@nanolab''
|'''233nm/min ±0.7%''' - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 ''by LN/BGHE@nanolab''
|-
|-
|PECVD1 (standard) oxide (5% load)
|PECVD1 (standard) oxide (5% load)
|'''242nm/min ±0.6%''' - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by ''LN/BGE@nanolab''
|'''242nm/min ±0.6%''' - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by ''LN/BGHE@nanolab''
|-
|-
|Silicon (10% load)
|Silicon (10% load)
Line 58: Line 60:
|
|
*34.2 nm/min (1:6 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech''
*34.2 nm/min (1:6 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech''
*50nm can be etched in 10min - [[/Etch of Al2O3|'''See results here''']] etched in November 2014 by ''FRSTO@danchip''
*50nm can be etched in 10min - [[/Etch of Al2O3|'''See results here''']] etched in November 2014 by ''Frederik Stöhr @danchip''
|-
|-
|Silicon rich nitride from furnace B2
|Silicon rich nitride from furnace B2
Line 65: Line 67:
|Cr
|Cr
|
|
6 nm/min (1:33 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech'' [http://process2share.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_SiO2 '''see here''']
6 nm/min (1:33 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech'' [[Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide#Dry_etch_with_Hard_mask|'''see here''']]
|-
|-
|Al
|Al
|
|
25nm/min (1:8 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech'' [http://process2share.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_SiO2 '''see here''']
25nm/min (1:8 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech'' [[Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide#Dry_etch_with_Hard_mask|'''see here''']]
|-
|-
|}
|}

Latest revision as of 17:44, 1 February 2023

Feedback to this page: click here

This page is written by Berit Herstrøm @ DTU Nanolab (BGHE) if nothing else is stated

The standard recipe

The standard recipe for oxide etching with photo resist as masking material is called: SiO2_res. The parameters and results so fare are as follows:

Parameter Recipe name: SiO2_res (SiO2 etch with resist mask)
Coil Power [W] 1300
Platen Power [W] 200
Platen temperature [oC] 0
He flow [sccm] 174
C4F8 flow [sccm] 5
H2 flow [sccm] 4
Pressure [mTorr] 4


Etch rates in different materials using the standard "Silicon oxide etch with resist mask"

Material to be etched Etch rate using SiO2_res
Thermal oxide
  • ~230nm/min (5% etch load) - etch load dependency see here
  • ~200 nm/min (100% etch load) fall 2016 by Martin Lind Ommen @nanotech see here
TEOS oxide (5% load) 233nm/min ±0.7% - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by LN/BGHE@nanolab
PECVD1 (standard) oxide (5% load) 242nm/min ±0.6% - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by LN/BGHE@nanolab
Silicon (10% load) 32-36 nm/min - January 2019 bghe@nanolab
Al2O3 from the ALD
  • 34.2 nm/min (1:6 to SiO2) fall 2016 by Martin Lind Ommen @nanotech
  • 50nm can be etched in 10min - See results here etched in November 2014 by Frederik Stöhr @danchip
Silicon rich nitride from furnace B2 136nm was etched in 1min (whole wafer) - etched in October 2015 by bghe@nanolab
Cr

6 nm/min (1:33 to SiO2) fall 2016 by Martin Lind Ommen @nanotech see here

Al

25nm/min (1:8 to SiO2) fall 2016 by Martin Lind Ommen @nanotech see here


Using different resist masks: results using the standard recipe for "Silicon oxide etch with resist mask"

. Az5214E MIR701 nLof KRF CSAR
Selectivity to thermal oxide [:1]
  • 2-3 - etch load dependency see here
  • 1.9 - tested November 2015 by BGHE
  • 2 - tested December 2022 by BGHE
1.8 - tested November 2015 by BGHE 2.0 - tested November 2015 by BGHE ~2 - tested May 2013 by Christian Østergaard @nanotech. .
Profile [o] ~90 - depends on the resist profile before etch, this was obtained with a negative process . . . .
Roughness of the resist after etch - striation on sidewalls see here see here see here . .
Images See here . . See images here .
Comments A negative resist process was done to make the mask. I have not had so good results with a positive resist process. . . . Using the standard oxide recipe (SiO2_res) for 1 min the CSAR looked burned and could not be removed by CSAR stripper (AR600-71). For a better recipe look here

Tried again (2016-08-19 bghe) with 1min with CSAR resist and this time it did not look burned.


Variations over the standard "SiO2 etch with resist mask" recipe

Parameter Recipe name: SiO2_res (SiO2 etch with resist mask) Variations over SiO2_res made in 2010 by BGHE
Coil Power [W] 1300 1000-1600
Platen Power [W] 200 150-300
Platen temperature [oC] 0 0
He flow [sccm] 174 174, 300
C4F8 flow [sccm] 5 5
H2 flow [sccm] 4 0, 4
Pressure [mTorr] 4 2.3, 4


Typical results Variations over SiO2_res made in 2010 by BGHE See results here
Etch rate of thermal oxide ~160-340nm/min
Selectivity to AZ resist [:1] 2.7-4.3
Profile angle 83-90
Images See here