Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using AOE/Standard recipe with resist mask: Difference between revisions
Jump to navigation
Jump to search
No edit summary |
|||
(25 intermediate revisions by 2 users not shown) | |||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide/SiO2_etch_using_AOE/Standard_recipe_with_resist_mask click here]''' | ||
{{CC-bghe1}} | |||
=The standard recipe= | =The standard recipe= | ||
Line 43: | Line 45: | ||
| | | | ||
*'''~230nm/min (5% etch load)''' - etch load dependency [[/AOE SiO2 etch load dependency|'''see here''']] | *'''~230nm/min (5% etch load)''' - etch load dependency [[/AOE SiO2 etch load dependency|'''see here''']] | ||
*~200 nm/min ''fall 2016 by Martin Lind Ommen @nanotech'' | *~200 nm/min (100% etch load) ''fall 2016 by Martin Lind Ommen @nanotech'' [[Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide#Dry_etch_with_Hard_mask|'''see here''']] | ||
|- | |- | ||
|TEOS oxide (5% load) | |TEOS oxide (5% load) | ||
|'''233nm/min ±0.7%''' - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 ''by LN/ | |'''233nm/min ±0.7%''' - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 ''by LN/BGHE@nanolab'' | ||
|- | |- | ||
|PECVD1 (standard) oxide (5% load) | |PECVD1 (standard) oxide (5% load) | ||
|'''242nm/min ±0.6%''' - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by ''LN/ | |'''242nm/min ±0.6%''' - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by ''LN/BGHE@nanolab'' | ||
|- | |||
|Silicon (10% load) | |||
|32-36 nm/min - January 2019 bghe@nanolab | |||
|- | |- | ||
|Al2O3 from the ALD | |Al2O3 from the ALD | ||
Line 55: | Line 60: | ||
| | | | ||
*34.2 nm/min (1:6 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech'' | *34.2 nm/min (1:6 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech'' | ||
*50nm can be etched in 10min - [[/Etch of Al2O3|'''See results here''']] etched in November 2014 by '' | *50nm can be etched in 10min - [[/Etch of Al2O3|'''See results here''']] etched in November 2014 by ''Frederik Stöhr @danchip'' | ||
|- | |- | ||
|Silicon rich nitride from furnace B2 | |Silicon rich nitride from furnace B2 | ||
|136nm was etched in 1min (whole wafer) - etched in October 2015 by ''bghe@ | |136nm was etched in 1min (whole wafer) - etched in October 2015 by ''bghe@nanolab'' | ||
|- | |- | ||
|Cr | |Cr | ||
|6 nm/min (1:33 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech'' | | | ||
6 nm/min (1:33 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech'' [[Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide#Dry_etch_with_Hard_mask|'''see here''']] | |||
|- | |- | ||
|Al | |Al | ||
|25nm/min (1:8 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech'' | | | ||
25nm/min (1:8 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech'' [[Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide#Dry_etch_with_Hard_mask|'''see here''']] | |||
|- | |- | ||
|} | |} | ||
Line 75: | Line 82: | ||
|-style="background:DarkGray; color:White" | |-style="background:DarkGray; color:White" | ||
!. | !. | ||
! | !Az5214E | ||
! | !MIR701 | ||
!nLof | !nLof | ||
!KRF | !KRF | ||
Line 85: | Line 92: | ||
*'''2-3''' - etch load dependency [[/AOE SiO2 etch load dependency|'''see here''']] | *'''2-3''' - etch load dependency [[/AOE SiO2 etch load dependency|'''see here''']] | ||
*'''1.9''' - ''tested November 2015 by BGHE'' | *'''1.9''' - ''tested November 2015 by BGHE'' | ||
*'''2''' - ''tested December 2022 by BGHE'' | |||
|'''1.8''' - ''tested November 2015 by BGHE'' | |'''1.8''' - ''tested November 2015 by BGHE'' | ||
|'''2.0''' - ''tested November 2015 by BGHE'' | |'''2.0''' - ''tested November 2015 by BGHE'' |
Latest revision as of 17:44, 1 February 2023
Feedback to this page: click here
This page is written by Berit Herstrøm @ DTU Nanolab (BGHE) if nothing else is stated
The standard recipe
The standard recipe for oxide etching with photo resist as masking material is called: SiO2_res. The parameters and results so fare are as follows:
Parameter | Recipe name: SiO2_res (SiO2 etch with resist mask) |
---|---|
Coil Power [W] | 1300 |
Platen Power [W] | 200 |
Platen temperature [oC] | 0 |
He flow [sccm] | 174 |
C4F8 flow [sccm] | 5 |
H2 flow [sccm] | 4 |
Pressure [mTorr] | 4 |
Etch rates in different materials using the standard "Silicon oxide etch with resist mask"
Material to be etched | Etch rate using SiO2_res |
---|---|
Thermal oxide | |
TEOS oxide (5% load) | 233nm/min ±0.7% - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by LN/BGHE@nanolab |
PECVD1 (standard) oxide (5% load) | 242nm/min ±0.6% - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by LN/BGHE@nanolab |
Silicon (10% load) | 32-36 nm/min - January 2019 bghe@nanolab |
Al2O3 from the ALD |
|
Silicon rich nitride from furnace B2 | 136nm was etched in 1min (whole wafer) - etched in October 2015 by bghe@nanolab |
Cr |
6 nm/min (1:33 to SiO2) fall 2016 by Martin Lind Ommen @nanotech see here |
Al |
25nm/min (1:8 to SiO2) fall 2016 by Martin Lind Ommen @nanotech see here |
Using different resist masks: results using the standard recipe for "Silicon oxide etch with resist mask"
. | Az5214E | MIR701 | nLof | KRF | CSAR |
---|---|---|---|---|---|
Selectivity to thermal oxide [:1] |
|
1.8 - tested November 2015 by BGHE | 2.0 - tested November 2015 by BGHE | ~2 - tested May 2013 by Christian Østergaard @nanotech. | . |
Profile [o] | ~90 - depends on the resist profile before etch, this was obtained with a negative process | . | . | . | . |
Roughness of the resist after etch - striation on sidewalls | see here | see here | see here | . | . |
Images | See here | . | . | See images here | . |
Comments | A negative resist process was done to make the mask. I have not had so good results with a positive resist process. | . | . | . | Using the standard oxide recipe (SiO2_res) for 1 min the CSAR looked burned and could not be removed by CSAR stripper (AR600-71). For a better recipe look here Tried again (2016-08-19 bghe) with 1min with CSAR resist and this time it did not look burned. |
Variations over the standard "SiO2 etch with resist mask" recipe
Parameter | Recipe name: SiO2_res (SiO2 etch with resist mask) | Variations over SiO2_res made in 2010 by BGHE |
---|---|---|
Coil Power [W] | 1300 | 1000-1600 |
Platen Power [W] | 200 | 150-300 |
Platen temperature [oC] | 0 | 0 |
He flow [sccm] | 174 | 174, 300 |
C4F8 flow [sccm] | 5 | 5 |
H2 flow [sccm] | 4 | 0, 4 |
Pressure [mTorr] | 4 | 2.3, 4 |
Typical results | Variations over SiO2_res made in 2010 by BGHE See results here |
---|---|
Etch rate of thermal oxide | ~160-340nm/min |
Selectivity to AZ resist [:1] | 2.7-4.3 |
Profile angle | 83-90 |
Images | See here |
Comments | . |