Line 81: | Line 81: | ||
File:contour plot for etchrate of slow etch in SiO2.JPG| Etch rate map of SiO2 etch on 6" wafer | File:contour plot for etchrate of slow etch in SiO2.JPG| Etch rate map of SiO2 etch on 6" wafer | ||
File:contour plot for etchrate of slow etch in SRN.JPG| Etch rate map of SRN etch on 6" wafer | File:contour plot for etchrate of slow etch in SRN.JPG| Etch rate map of SRN etch on 6" wafer | ||
</gallery> | |||
<gallery caption="Map of etch rate measurements for 'Slow Etch2'" widths="300px" heights="300px" perrow="2"> | |||
File:Contour Plot etch rates Si3N4.jpg| Etch rate map of Si3N4 etch on 4" wafer (on 6" carrier) | |||
File:Contour Plot etch rates SRN.jpg| Etch rate map of SRN etch on 4" wafer (on 6" carrier) | |||
File:Contour Plot etch rates SiO2.jpg|Etch rate map of SiO2 etch on 4" wafer (on 6" carrier) | |||
File:Contour Plot etch rates Si.jpg|Etch rate map of Si etch on 4" wafer (on 6" carrier) | |||
</gallery> | </gallery> |
Revision as of 13:55, 27 January 2023
The slow etch
This work is done by Berit Herstrøm @Nanolab.dtu, is nothing else is stated The slow etch is designed to etch slow at low powers to etch thin films and to avoid overheating of samples mounted on a carrier with Capton/polyimide tape
Parameter | Recipe name: Slow Etch | Recipe name: Slow Etch2 |
---|---|---|
Coil Power [W] | 350 | 200 |
Platen Power [W] | 25 | 50 |
Platen temperature [oC] | 20 | 20 |
H2 flow [sccm] | 15 | 15 |
CF4 flow [sccm] | 30 | 30 |
Pressure [mTorr] | 3 | 10 |
Typical results | Slow Etch | Slow Etch2 |
---|---|---|
Etch of SRN | ~43nm/min [measured 39-50 nm/min over a 6" wafer] | 23-25 nm/min [4" on carrier]] |
Etch rate of Si3N4 | ~49 nm/min [4" on carrier] | 24-26 nm/min [4" on carrier] |
Etch rate of SiO2 | ~42nm/min [41-43 nm/min over a 6" wafer] | 13.7-14.7 nm/min [4" on carrier] |
Etch rate of Mir resist] | ~nm/min | ~17 nm/min |
Tested etch time without burning the resist | 3 min | 30 min |
Profile [o] |