=The slow etch=  
=The slow etch=  
''This work is done by Berit Herstrøm @Nanolab.dtu, is nothing else is stated''
The slow etch is designed to etch slow at low powers to etch thin films and to avoid overheating of samples mounted on a carrier with Capton/polyimide tape
The slow etch is designed to etch slow at low powers to etch thin films and to avoid overheating of samples mounted on a carrier with Capton/polyimide tape



Revision as of 09:56, 27 January 2023

The slow etch

This work is done by Berit Herstrøm @Nanolab.dtu, is nothing else is stated The slow etch is designed to etch slow at low powers to etch thin films and to avoid overheating of samples mounted on a carrier with Capton/polyimide tape

Parameter Recipe name: Slow Etch Recipe name: Slow Etch2
Coil Power [W] 350 200
Platen Power [W] 25 50
Platen temperature [oC] 20 20
H2 flow [sccm] 15 15
CF4 flow [sccm] 30 30
Pressure [mTorr] 3 10
Typical results Slow Etch Slow Etch2
Etch of SRN ~43nm/min [measured 39-50 nm/min over a 6" wafer]
Etch rate of Si3N4 ~49nm/min [4" on carrier]
Etch rate of SiO2 ~42nm/min [41-43 nm/min over a 6" wafer]
Etch rate of DUV resist] ~nm/min


Profile [o]