Specific Process Knowledge/Thin film deposition/Deposition of Tungsten/Evaporation of W in Temescal: Difference between revisions

From LabAdviser
Eves (talk | contribs)
No edit summary
Eves (talk | contribs)
No edit summary
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition of Tungsten/Evaporation of W in Temescal click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Tungsten/Evaporation_of_W_in_Temescal click here]'''


=Deposition of W in Temescal=
=Deposition of W in Temescal=

Revision as of 16:12, 2 January 2023

Feedback to this page: click here

Deposition of W in Temescal

During the e-beam deposition of Tungsten, extremely bright light and heat are generated! Lower density film than expected due to porosity. Consider using sputtering instead.

Power 33W, stable rate, tooling 86%. Measured thickness 20 nm (XRR).

Wait for base pressure 3 10-7Torr before start.


Deposition of Tungsten. Dep. rate: 0.5Å/s, Thickness sp.: 20nm
Tooling factor 86% 2022-02-25
Layer name Thickness (nm) Density (g/cm3) Rougness (nm) Delta Beta
Moisture 0.80 0.52 0.52 1.7906e-6 4.1579e-8
WOx

1.01

5.00 0.72 1.6991e-5 3.9456e-7
W

19.12

15.66 0.81 3.7045e-5 2.9324e-6
SiO2 (native oxide) 2.09 2.15 0.32 7.0136e-6 1.6287e-7
Si (wafer) 2.33 0.00 7.5860e-6 1.7616e-7