Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/Slow etch: Difference between revisions
< Specific Process Knowledge | Etch | DRIE-Pegasus | Pegasus-4
Jump to navigation
Jump to search
Line 62: | Line 62: | ||
<br clear="all" /> | <br clear="all" /> | ||
<gallery caption="Map of etch rate measurements" widths=" | <gallery caption="Map of etch rate measurements" widths="300px" heights="300px" perrow="2"> | ||
File:contour plot for etchrate of slow etch in SiO2.JPG| Etch rate map of SiO2 etch on 6" wafer | File:contour plot for etchrate of slow etch in SiO2.JPG| Etch rate map of SiO2 etch on 6" wafer | ||
File:contour plot for etchrate of slow etch in SRN.JPG| Etch rate map of SRN etch on 6" wafer | File:contour plot for etchrate of slow etch in SRN.JPG| Etch rate map of SRN etch on 6" wafer | ||
</gallery> | </gallery> |
Revision as of 16:54, 6 December 2022
The slow etch
The slow etch is designed to etch slow at low powers to etch thin films and to avoid overheating of samples mounted on a carrier with Capton/polyimide tape
Parameter | Recipe name: Slow Etch |
---|---|
Coil Power [W] | 350 |
Platen Power [W] | 25 |
Platen temperature [oC] | 20 |
He flow [sccm] | 0 |
CF4 flow [sccm] | 45 |
Pressure [mTorr] | 3 |
Typical results | Test Results |
---|---|
Etch of SRN | ~43nm/min [measured 39-50 nm/min over a 6" wafer] |
Etch rate of Si3N4 | ~49nm/min [4" on carrier] |
Etch rate of SiO2 | ~42nm/min [41-43 nm/min over a 6" wafer] |
Etch rate of DUV resist] | ~nm/min
|
Profile [o] |