The slow etch

The slow etch is designed to etch slow at low powers to etch thin films and to avoid overheating of samples mounted on a carrier with Capton/polyimide tape

Parameter Recipe name: Slow Etch
Coil Power [W] 350
Platen Power [W] 25
Platen temperature [oC] 20
He flow [sccm] 0
CF4 flow [sccm] 45
Pressure [mTorr] 3
Typical results Test Results
Etch of SRN ~43nm/min [measured 39-50 nm/min over a 6" wafer]
Etch rate of Si3N4 ~49nm/min [4" on carrier]
Etch rate of SiO2 ~42nm/min [41-43 nm/min over a 6" wafer]
Etch rate of DUV resist] ~nm/min


Profile [o]