Specific Process Knowledge/Etch/Etching of Polymer/Etch of Photo Resist using RIE: Difference between revisions
Jump to navigation
Jump to search
No edit summary |
|||
(2 intermediate revisions by one other user not shown) | |||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Polymer/Etch_of_Photo_Resist_using_RIE click here]''' | ||
=<span style="color:#FF0000"> Both RIE's (RIE1 and RIE2) for silicon based etching has been decommissioned </span> = | =<span style="color:#FF0000"> Both RIE's (RIE1 and RIE2) for silicon based etching has been decommissioned </span> = | ||
* <span style="color:#FF0000"> This information is save because it might be valuable as inspiration for other dry etch systems. | |||
For a general introduction to RIE at | For a general introduction to RIE at Nanolab see [[Specific Process Knowledge/Etch/RIE (Reactive Ion Etch)|RIE (Reactive Ion Etch)]] | ||
Etching of polymer using RIE should only be done if you have no other options. The reason for this is that we want to keep our RIE's as clean as possible. However it can be used for stripping your resist after an etch if you need to keep your sample clean or you need to remove a very thin layer of resist before a RIE etch - like a descum. The process for etching away photoresist or other polymers involves an O2 plasma.Our standard cleaning recipe has been tested for a load of 50% resist on a wafer. | Etching of polymer using RIE should only be done if you have no other options. The reason for this is that we want to keep our RIE's as clean as possible. However it can be used for stripping your resist after an etch if you need to keep your sample clean or you need to remove a very thin layer of resist before a RIE etch - like a descum. The process for etching away photoresist or other polymers involves an O2 plasma.Our standard cleaning recipe has been tested for a load of 50% resist on a wafer. |
Latest revision as of 13:18, 6 September 2022
Feedback to this page: click here
Both RIE's (RIE1 and RIE2) for silicon based etching has been decommissioned
- This information is save because it might be valuable as inspiration for other dry etch systems.
For a general introduction to RIE at Nanolab see RIE (Reactive Ion Etch)
Etching of polymer using RIE should only be done if you have no other options. The reason for this is that we want to keep our RIE's as clean as possible. However it can be used for stripping your resist after an etch if you need to keep your sample clean or you need to remove a very thin layer of resist before a RIE etch - like a descum. The process for etching away photoresist or other polymers involves an O2 plasma.Our standard cleaning recipe has been tested for a load of 50% resist on a wafer.
Some RIE recipes for etching of silicon nitride:
Name | O2 flow | N2 flow | Pressure | Power |
---|---|---|---|---|
clean05 | 99 sccm | 20 sccm | 300 mTorr | 100 W |
Expected result using the above RIE recipes for etching of photoresist:
You should be aware that the result can deviate quit a lot from what is written here depending on ex. the mask loading.
Name | Tested with mask load: | Etch rate | Comments |
---|---|---|---|
Clean05 on RIE2 | 50% | ~740 nm/min | without being exposed to RIE before the photoresist etch |