Specific Process Knowledge/Thin film deposition/ALD Picosun R200/ZnO deposition using ALD: Difference between revisions
No edit summary |
No edit summary |
||
Line 4: | Line 4: | ||
Deposition of ZnO is a standard, well-explored ALD process. | |||
Previously (before 2018), DEZ had its independent inlet (A1), which shared the same N2 line with the TiCl4 precursor (A2). The DEZ precursor bottle was placed in a cabinet behind the instrument in the service area, and a long pipe led the precursor to the ALD chamber. This option has been abandoned due to safety reasons. This line was very difficult to purge in case of service. The results that were obtained with the old hardware configuration now remain obsolete. | |||
Nowadays, if the user wants to deposit ZnO, in ALD-1 the diethyl zinc (DEZ) has to be mounted in the A-line. If TiCl4 is currently present it has to be exchanged with DEZ. This is a time-consuming job, that needs to be ordered and prepared in advance. | |||
=ZnO ALD deposition | =ZnO ALD deposition using DEZ and H<sub>2</sub>O= | ||
< | |||
<b>Recipe: ZnOT</b> | ZnO can be deposited in the range between 100 <sup>o</sup>C to 225 <sup>o</sup>C. It is not recommended to increase the temperature above 225<sup>o</sup>C, as the uniformity suffers due to the precursor decomposition. The maximum temperature can be 250<sup>o</sup>C, here however the film crystal quality, crystallinity, roughness, etc. sufficiently differ from the films prepared in a lower temperature range. | ||
All results shown on this page have been obtained using the present (from 2018) configuration. | |||
Deposition and characterization has been performed in <b>2021 by Evgeniy Shkondin, DTU Nanolab</b> | |||
=ZnO recipes= | |||
==<b>Recipe: ZnO</b>== | |||
<b>Maximum deposition thickness: 100 nm</b> | |||
<b>Temperature: 100 <sup>o</sup>C - 250 <sup>o</sup>C</b> | |||
{| border="2" cellspacing="2" cellpadding="5" align="none" | |||
|- | |||
| | |||
!DEZ* | |||
!H<sub>2</sub>O | |||
|- | |||
!Nitrogen flow | |||
|150 sccm | |||
|200 sccm | |||
|- | |||
!Pulse time | |||
|0.1 s | |||
|0.1 s | |||
|- | |||
!Purge time | |||
|5.0 s | |||
|5.0 s | |||
|- | |||
|} | |||
This is a standard recipe of ZnO. It is suitable for coating the flat samples and structures with an aspect ratio of around up to 1:10. | |||
==<b>Recipe: ZnOT</b>== | |||
<b>Maximum deposition thickness: 100 nm</b> | <b>Maximum deposition thickness: 100 nm</b> | ||
Line 45: | Line 80: | ||
|- | |- | ||
|} | |} | ||
<br clear="all" /> | |||
This is a more complicated recipe that allows coating the sample with very high aspect ratio profiles. One SEM example is shown on one of the images below. The recipe is good for deposition on very high aspect ratio structures (with aspect ratio more than 1:20) such as deep trenches, pillars, pores etc. <b>ZnOT</b> recipe can also be used for deposition on polymers at low temperatures (80-120 <sup>o</sup>C). | |||
<br clear="all" /> | |||
<strong>DEZ</strong> is diethylzinc Zn(CH<sub>2</sub>CH<sub>3</sub>)<sub>2</sub> or ZnEt<sub>2</sub> | <strong>DEZ</strong> is diethylzinc Zn(CH<sub>2</sub>CH<sub>3</sub>)<sub>2</sub> or ZnEt<sub>2</sub> | ||
<br clear="all" /> | <br clear="all" /> | ||
= | =Deposition characteristics= | ||
The deposition rate for ZnO depends on the temperature, see the ALD-window graph below. The uniformity, thickness, refractive index has been obtained using | The deposition rate for ZnO depends on the temperature, see the ALD-window graph below. The uniformity, thickness, refractive index has been obtained using Ellipsometer VASE. | ||
==Deposition rate== | |||
<gallery caption="" widths=" | In the graphs below the ZnO thickness vs. number of cycles for deposition temperatures between 100 <sup>o</sup>C and 250 <sup>o</sup>C presented. Results have been obtained for <100> 100 mm Si wafers with native oxide, based on ellipsometry study. | ||
image: | |||
image: | <gallery caption="" widths="400px" heights="400px" perrow="2"> | ||
image:eves_dep_rate_ZnO_100C_ALD1_20220223.png|Deposition rate of ZnO at 100 <sup>o</sup>C. Substrate: Silicon 4" wafer with native oxide. <br> <math> Thickness (nm) = 0.1483 \cdot N + 0.63 </math> | |||
image:eves_dep_rate_ZnO_150C_ALD1_20220223.png|Deposition rate of ZnO at 150 <sup>o</sup>C. Substrate: Silicon 4" wafer with native oxide. <br> <math> Thickness (nm) = 0.1954 \cdot N - 2.73 </math> | |||
image:eves_dep_rate_ZnO_200C_ALD1_20220223.png|Deposition rate of ZnO at 200 <sup>o</sup>C. Substrate: Silicon 4" wafer with native oxide. <br> <math> Thickness (nm) = 0.1842 \cdot N - 3.80 </math> | |||
image:eves_dep_rate_ZnO_250C_ALD1_20220223.png|Deposition rate of ZnO at 250 <sup>o</sup>C. Substrate: Silicon 4" wafer with native oxide. <br> <math> Thickness (nm) = 0.1326 \cdot N + 1.13 </math> | |||
image:eves_ALD_window_ZnO_ALD1_20220223.png|ALD window of ZnO | |||
</gallery> | </gallery> | ||
<br clear="all" /> | <br clear="all" /> | ||
< | ==Uniformity across 100 mm wafer== | ||
< | |||
Recipe "ZnO" Samples: 100mm ssp-Si | |||
{| border="2" cellspacing="0" cellpadding="9" | |||
!colspan="1" border="none" style="background:silver; color:black;" align="center"|Temperature (°C) / Number of cycles | |||
|style="background:silver; color:black"|<b>Deposition rate (nm/s)</b> | |||
|style="background:silver; color:black"|<b>Average thickness (nm)</b> | |||
|style="background:silver; color:black"|<b>Standard deviation</b> | |||
|style="background:silver; color:black"|<b>Uniformity (%)</b> | |||
|- | |||
!style="background:silver; color:black;" align="center" |100°C / 500cycles | |||
|style="background:WhiteSmoke; color:black" align="center"|<b><span style="color: red">0.1483</span></b> | |||
|style="background:WhiteSmoke; color:black" align="center"|75.67 | |||
|style="background:WhiteSmoke; color:black" align="center"|1.49 | |||
|style="background:WhiteSmoke; color:black" align="center"|3.26 | |||
|- | |||
!style="background:silver; color:black;" align="center" |150°C / 500cycles | |||
|style="background:WhiteSmoke; color:black" align="center"|<b><span style="color: red">0.1954</span></b> | |||
|style="background:WhiteSmoke; color:black" align="center"|95.32 | |||
|style="background:WhiteSmoke; color:black" align="center"|1.32 | |||
|style="background:WhiteSmoke; color:black" align="center"|2.44 | |||
|- | |||
!style="background:silver; color:black;" align="center" |200°C / 500cycles | |||
|style="background:WhiteSmoke; color:black" align="center"|<b><span style="color: red">0.1842</span></b> | |||
|style="background:WhiteSmoke; color:black" align="center"|87.97 | |||
|style="background:WhiteSmoke; color:black" align="center"|0.31 | |||
|style="background:WhiteSmoke; color:black" align="center"|0.63 | |||
|- | |||
!style="background:silver; color:black;" align="center" |225°C / 500cycles | |||
|style="background:WhiteSmoke; color:black" align="center"|<b><span style="color: red">0.1622</span></b> | |||
|style="background:WhiteSmoke; color:black" align="center"|81.09 | |||
|style="background:WhiteSmoke; color:black" align="center"|0.45 | |||
|style="background:WhiteSmoke; color:black" align="center"|1.07 | |||
|- | |||
!style="background:silver; color:black;" align="center" |250°C / 500cycles | |||
|style="background:WhiteSmoke; color:black" align="center"|<b><span style="color: red">0.1326</span></b> | |||
|style="background:WhiteSmoke; color:black" align="center"|67.92 | |||
|style="background:WhiteSmoke; color:black" align="center"|1.71 | |||
|style="background:WhiteSmoke; color:black" align="center"|3.82 | |||
|- | |||
|} | |||
<br> | |||
<!-- --> | |||
<gallery caption="" widths="400px" heights="400px" perrow="3"> | |||
image:eves_SE_uniformity_ZnO_100C_ALD1_20220223.png|Uniformity across 100mm wafer. Deposition at 100°C | |||
image:eves_SE_uniformity_ZnO_150C_ALD1_20220223.png|Uniformity across 100mm wafer. Deposition at 150°C | |||
image:eves_SE_uniformity_ZnO_200C_ALD1_20220223.png|Uniformity across 100mm wafer. Deposition at 200°C | |||
image:eves_SE_uniformity_ZnO_225C_ALD1_20220223.png|Uniformity across 100mm wafer. Deposition at 225°C | |||
image:eves_SE_uniformity_ZnO_250C_ALD1_20220223.png|Uniformity across 100mm wafer. Deposition at 250°C | |||
</gallery> | |||
=Optical functions= | |||
<gallery caption="" widths="400px" heights="400px" perrow="2"> | |||
image:eves_ref_index_ZnO_ALD1_20220223.png|Refractive index. | |||
image:eves_abs_coeff_ZnO_ALD1_20220223.png|Absorption coefficient. | |||
</gallery> | |||
=SEM images= | |||
<gallery caption="" widths=" | <gallery caption="" widths="400px" heights="400px" perrow="3"> | ||
image: | image:eves_SEM_ZnO_500cycles_100C_ALD1_20220223_convert.png|SEM image of flat surface of ZnO. Deposition at 100°C | ||
image:eves_SEM_ZnO_500cycles_150C_ALD1_20220223_convert.png|SEM image of flat surface of ZnO. Deposition at 150°C | |||
image:eves_SEM_ZnO_500cycles_200C_ALD1_20220223_convert.png|SEM image of flat surface of ZnO. Deposition at 200°C | |||
image:eves_SEM_ZnO_500cycles_225C_ALD1_20220223_convert.png|SEM image of flat surface of ZnO. Deposition at 225°C | |||
image:eves_SEM_ZnO_500cycles_250C_ALD1_20220223_convert.png|SEM image of flat surface of ZnO. Deposition at 250°C | |||
image:eves_SEM_ZnO_HARS_ALD1_20220223_convert.png|ZnO deposition example on high aspect ratio structures. "<b>ZnOT</b>" recipe was used. | |||
</gallery> | </gallery> | ||
=ZnO XPS investigation for elemental trace analysis= | |||
< | |||
< | XPS profile for ZnO has been obtained using XPs K-alpha. ZnO samples reveals chemically high quality films with no observable contaminations in temperature range 100 - 250 <sup>o</sup>C. | ||
< | |||
<gallery caption="" widths="600px" heights="600px" perrow="1"> | |||
image:eves_ALD1_XPS_ZnO_20220223.png|XPS survey scan of ZnO. | |||
</gallery> |
Revision as of 12:12, 4 March 2022
Feedback to this page: click here
This page presents new data. The old results can be foud in Obsolete page
Deposition of ZnO is a standard, well-explored ALD process. Previously (before 2018), DEZ had its independent inlet (A1), which shared the same N2 line with the TiCl4 precursor (A2). The DEZ precursor bottle was placed in a cabinet behind the instrument in the service area, and a long pipe led the precursor to the ALD chamber. This option has been abandoned due to safety reasons. This line was very difficult to purge in case of service. The results that were obtained with the old hardware configuration now remain obsolete. Nowadays, if the user wants to deposit ZnO, in ALD-1 the diethyl zinc (DEZ) has to be mounted in the A-line. If TiCl4 is currently present it has to be exchanged with DEZ. This is a time-consuming job, that needs to be ordered and prepared in advance.
ZnO ALD deposition using DEZ and H2O
ZnO can be deposited in the range between 100 oC to 225 oC. It is not recommended to increase the temperature above 225oC, as the uniformity suffers due to the precursor decomposition. The maximum temperature can be 250oC, here however the film crystal quality, crystallinity, roughness, etc. sufficiently differ from the films prepared in a lower temperature range.
All results shown on this page have been obtained using the present (from 2018) configuration.
Deposition and characterization has been performed in 2021 by Evgeniy Shkondin, DTU Nanolab
ZnO recipes
Recipe: ZnO
Maximum deposition thickness: 100 nm
Temperature: 100 oC - 250 oC
DEZ* | H2O | |
---|---|---|
Nitrogen flow | 150 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s |
Purge time | 5.0 s | 5.0 s |
This is a standard recipe of ZnO. It is suitable for coating the flat samples and structures with an aspect ratio of around up to 1:10.
Recipe: ZnOT
Maximum deposition thickness: 100 nm
Temperature: 100 oC - 250 oC
DEZ* | DEZ | H2O | H2O | |
---|---|---|---|---|
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
This is a more complicated recipe that allows coating the sample with very high aspect ratio profiles. One SEM example is shown on one of the images below. The recipe is good for deposition on very high aspect ratio structures (with aspect ratio more than 1:20) such as deep trenches, pillars, pores etc. ZnOT recipe can also be used for deposition on polymers at low temperatures (80-120 oC).
DEZ is diethylzinc Zn(CH2CH3)2 or ZnEt2
Deposition characteristics
The deposition rate for ZnO depends on the temperature, see the ALD-window graph below. The uniformity, thickness, refractive index has been obtained using Ellipsometer VASE.
Deposition rate
In the graphs below the ZnO thickness vs. number of cycles for deposition temperatures between 100 oC and 250 oC presented. Results have been obtained for <100> 100 mm Si wafers with native oxide, based on ellipsometry study.
Uniformity across 100 mm wafer
Recipe "ZnO" Samples: 100mm ssp-Si
Temperature (°C) / Number of cycles | Deposition rate (nm/s) | Average thickness (nm) | Standard deviation | Uniformity (%) |
---|---|---|---|---|
100°C / 500cycles | 0.1483 | 75.67 | 1.49 | 3.26 |
150°C / 500cycles | 0.1954 | 95.32 | 1.32 | 2.44 |
200°C / 500cycles | 0.1842 | 87.97 | 0.31 | 0.63 |
225°C / 500cycles | 0.1622 | 81.09 | 0.45 | 1.07 |
250°C / 500cycles | 0.1326 | 67.92 | 1.71 | 3.82 |
Optical functions
SEM images
ZnO XPS investigation for elemental trace analysis
XPS profile for ZnO has been obtained using XPs K-alpha. ZnO samples reveals chemically high quality films with no observable contaminations in temperature range 100 - 250 oC.