Specific Process Knowledge/Thin film deposition/ALD Picosun R200/ZnO deposition using ALD: Difference between revisions
No edit summary |
|||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200/ZnO_deposition_using_ALD click here]''' | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200/ZnO_deposition_using_ALD click here]''' | ||
This page presents new data. The old results can be foud in [[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200/ZnO deposition using ALD/Obsolete|Obsolete page]] | |||
The ALD window for deposition of zinc oxide (ZnO) ranges from 100 <sup>o</sup>C to 250 <sup>o</sup>C. Several investigation techniques has been implemented for ZnO characterization. Additionally, more information on ZnO can be found on a page about [[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200/AZO_deposition_using_ALD|Al-doped ZnO (AZO)]] | The ALD window for deposition of zinc oxide (ZnO) ranges from 100 <sup>o</sup>C to 250 <sup>o</sup>C. Several investigation techniques has been implemented for ZnO characterization. Additionally, more information on ZnO can be found on a page about [[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200/AZO_deposition_using_ALD|Al-doped ZnO (AZO)]] |
Revision as of 12:10, 4 March 2022
Feedback to this page: click here
This page presents new data. The old results can be foud in Obsolete page
The ALD window for deposition of zinc oxide (ZnO) ranges from 100 oC to 250 oC. Several investigation techniques has been implemented for ZnO characterization. Additionally, more information on ZnO can be found on a page about Al-doped ZnO (AZO)
All results shown on this page have been obtained using the "ZnOT" recipe on new Si(100) wafers with native oxide:
ZnO ALD deposition
Evgeniy Shkondin, DTU Danchip, 2014-2016.
ZnO standard recipe
Recipe: ZnOT
Maximum deposition thickness: 100 nm
Temperature: 100 oC - 250 oC
DEZ* | DEZ | H2O | H2O | |
---|---|---|---|---|
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
DEZ is diethylzinc Zn(CH2CH3)2 or ZnEt2
ZnO deposition rates and uniformity
The deposition rate for ZnO depends on the temperature, see the ALD-window graph below. The uniformity, thickness, refractive index has been obtained using Ellipsometer VASE.
ZnO XPS investigation for elemental trace analysis and deposition on high aspect ratio structures
XPS profile for ZnO has been obtained using XPS K-Alpha. ZnO samples reveals (see Figure 3a) chemically high quality films with no observable contaminations in temperature range 100 - 250 oC.
The recipe is good for deposition on very high aspect ratio structures (with aspect ratio more than 1:20) such as deep trenches, pillars, pores etc. ZnOT recipe can also be used for deposition on polymers at low temperatures (80-120 oC).
Figure 3. a) XPS survey scan b) SEM images of ZnO deposited on a Si trenches at 200 oC temperature and 700 cycles. Trenches prepered using DRIE-Pegasus. Inset image shows the photography of the sample.
Evgeniy Shkondin, DTU Danchip, 2014-2016.