Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/isotropic: Difference between revisions
No edit summary |
|||
(2 intermediate revisions by one other user not shown) | |||
Line 1: | Line 1: | ||
= Isotropic etching in silicon on the ICP Metal Etch = | = Isotropic etching in silicon on the ICP Metal Etch = | ||
<!--Checked for updates on 11/2-2019 - ok/jmli --> | <!--Checked for updates on 11/2-2019 - ok/jmli --> | ||
<!--Checked for updates on 24/8-2021. ok/ jmli--> | |||
{| border="1" cellpadding="0" cellspacing="0" style="text-align:center;" | {| border="1" cellpadding="0" cellspacing="0" style="text-align:center;" | ||
Line 50: | Line 50: | ||
| 3 <!--Platen power --> | | 3 <!--Platen power --> | ||
| [[Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/isotropic/isoslow1|'''Click HERE!''' ]] <!-- link processes --> | | [[Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/isotropic/isoslow1|'''Click HERE!''' ]] <!-- link processes --> | ||
| | | Note: Lior Shiv got very high etch rate for this recipe >1.5µm/min 2019-07-12 <!--Keywords --> | ||
|- | |- | ||
|- | |- | ||
! no name, tested by Lior Shiv@Capres 2019- | ! no name, tested by Lior Shiv@Capres 2019-07-12 <!--Recipe Name --> | ||
| A <!--Step --> | | A <!--Step --> | ||
| 20 <!--Temperature --> | | 20 <!--Temperature --> |
Latest revision as of 16:20, 24 August 2021
Isotropic etching in silicon on the ICP Metal Etch
Recipe | Step | Temp. | Time | Pres. | Hardware | Gasses | RF powers | Observations | |||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
SF6 | O2 | C4F8 | Ar | CF4 | H2 | CH4 | BCl3 | Cl2 | HBr | Coil | Platen | SEM images of different runs | Keywords | ||||||
isoslow1 | A | 20 | - | 10 | - | 90 | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 400 | 3 | Click HERE! | Note: Lior Shiv got very high etch rate for this recipe >1.5µm/min 2019-07-12 |
no name, tested by Lior Shiv@Capres 2019-07-12 | A | 20 | - | 10 | - | 90 | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 150 | 3 | About 10% load, etch rate around 400nm/min |