=== GaAs nano etch === | === GaAs nano etch === | ||
Line 29: | Line 29: | ||
{| border="1" cellspacing="2" cellpadding="3" align="left" | {| border="1" cellspacing="2" cellpadding="3" align="left" | ||
|colspan="2" align="center"| '''Results (GaAs Nano Etch)''' | |colspan="2" align="center"| '''Results (GaAs Nano Etch)''' ''from 2011 by Thor Ansbæk @photonic'' | ||
|- | |- | ||
|GaAs | |GaAs |
Latest revision as of 14:42, 18 August 2021
Feedback to this page: click here
GaAs nano etch
Recipe | GaAs Nano Etch |
Cl2 flow | 4 sccm |
Ar flow | 12 sccm |
Platen power | 80 W |
Coil power | 700 W |
Pressure | 6 mTorr |
Platen chiller temperature | 20 oC |
Results (GaAs Nano Etch) from 2011 by Thor Ansbæk @photonic | |
GaAs | 5 nm/s |
AlInP | 1 nm/s |
HSQ | 1.5 nm/s |
ZEP520a | 2 nm/s |
Si3N4 | 2 nm/s |