Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using AOE/Standard recipe with resist mask/Etch of Al2O3: Difference between revisions
< Specific Process Knowledge | Etch | Etching of Silicon Oxide | SiO2 etch using AOE | Standard recipe with resist mask
Jump to navigation
Jump to search
No edit summary |
|||
Line 5: | Line 5: | ||
''by Fredrik Stöhr@danchip.dtu.dk'' | ''by Fredrik Stöhr@danchip.dtu.dk'' | ||
Aluminum oxide (Al<sub>2</sub>O<sub>3</sub>, Alumina) can be etched with the standard recipe for silicon oxide etching. The parameters including the chuck temperature are identical to the recipe described above: '''SiO2_res'''. ''The etch is probably very physical and gives redeposition, so please | Aluminum oxide (Al<sub>2</sub>O<sub>3</sub>, Alumina) can be etched with the standard recipe for silicon oxide etching. The parameters including the chuck temperature are identical to the recipe described above: '''SiO2_res'''. <br> | ||
'''The etch is probably very physical and gives redeposition, so please using a Cl2 etch on the ICP metal instead (BGHE 2015-04-17)''' <br> | |||
'''General Description'''<br> | '''General Description'''<br> |
Revision as of 14:49, 18 August 2021
Feedback to this page: click here
Etching of micro structures in Aluminum oxide using the standard SiO2 recipe
by Fredrik Stöhr@danchip.dtu.dk
Aluminum oxide (Al2O3, Alumina) can be etched with the standard recipe for silicon oxide etching. The parameters including the chuck temperature are identical to the recipe described above: SiO2_res.
The etch is probably very physical and gives redeposition, so please using a Cl2 etch on the ICP metal instead (BGHE 2015-04-17)
General Description
- Process date: Summer 2014
- Aluminum Oxide with a thickness of 50 nm has been deposited by atomic layer deposition using the respective standard recipe.
- Substrates: Blank 525 µm Silicon wafers or Silicon wafers with thermally grown Silicon Oxide prior to Alumina deposition.
- Mask: [XOP8] AZ5214E 1.5 µm thick (HMDS pretreatment, 6-inch aligner 3 sec exposure, 60 sec development).
- Etch Load (Total Exposed SiO2): ~ 5 %
- Post process: O2 Plasma Ashing 10 min