<gallery caption="Recipe no. 10: C06445_02 coil_2500W, platen:300W, He/C4F8= 17.5, C4F8/H2=1, Pressure:8.8mTorr, C4F8:25.6sccm, He:448.7sccm, H2:25.6sccm, 3:56 min " perrow=" | <gallery caption="Recipe no. 10: C06445_02 coil_2500W, platen:300W, He/C4F8= 17.5, C4F8/H2=1, Pressure:8.8mTorr, C4F8:25.6sccm, He:448.7sccm, H2:25.6sccm, 3:56 min " perrow="4"> | ||
Image:C06445_02_11.jpg|0.4µ/0.2µ<br> Bad lithography | Image:C06445_02_11.jpg|0.4µ/0.2µ<br> Bad lithography |
Revision as of 09:34, 5 February 2021
SiO2 Etch
I am in the process of doing some development of a SiO2 etch. So far I have found this fairly good recipe. For now it is the standard SiO2 etch recipes but I might change the "Standard recipe" a a later time if I find a better one. You are welcome to contact me see more result. I will add them to Labadviser at a later time. /Berit Herstrøm bghe@dtu.dk (Nanolab)
- Recipe no. 10: C06445_02 coil_2500W, platen:300W, He/C4F8= 17.5, C4F8/H2=1, Pressure:8.8mTorr, C4F8:25.6sccm, He:448.7sccm, H2:25.6sccm, 3:56 min