Specific Process Knowledge/Thin film deposition/DiamondCVD/Diamond CVD process details: Difference between revisions
(new page on diamond process) |
|||
Line 10: | Line 10: | ||
[[File:diamond example.png|upright=2.5|alt=Two-inch wafer that has a speckled dark gray appearance with three small transparent partly overlapping squares in one area on top. The wafer is labeled as "polycrystalline diamond substrate" and the squares are labeled as "single crystal diamond" |right|thumb|Single- and polycrystalline diamond]] | [[File:diamond example.png|upright=2.5|alt=Two-inch wafer that has a speckled dark gray appearance with three small transparent partly overlapping squares in one area on top. The wafer is labeled as "polycrystalline diamond substrate" and the squares are labeled as "single crystal diamond" |right|thumb|Single- and polycrystalline diamond]] | ||
It is possible to grow | ===Single crystal diamond=== | ||
It is possible to grow very clean diamond in the SEKI system. In theory it would even be possible to control the N<sub>2</sub> dopant level and dopant depth. However, in practice it would be necessary to have our own hydrogen generator or to buy (very expensive) extra pure hydrogen to make this possible. The hydrogen we have for general processing at Nanolab simply contains too much nitrogen. To control doping levels it is necessary to use 7N hydrogen and to mix it with a very small additional flow of hydrogen mixed with only a few percent nitrogen. | |||
For | Nitrogen doping affects the optical and electronic properties of the diamond. For instance this can be used in magnetic sensors, which is a topic of research at DTU Physics. | ||
Polishing is needed after deposition if the polycrystalline diamond layer has to be smooth. Thinning is needed if the diamond layer has to be very thin as a uniform diamond layer can only be deposited above 1 μm thickness. | It is possible to grow single crystal diamond in the SEKI by using a single crystalline diamond substrate (these are purchased and typical dimensions might be 2x2 mm with 0.1 mm thickness). We have not investigated whether it is possible to distinguish the transition from the purchased substrate to the newly grown layer. | ||
===Polycrystalline diamond=== | |||
For polycrystalline growth the substrate must be seeded with diamonds. This is commonly done by sonicating the substrate in a solution of water with nano diamonds, although other solvents may give better results ([https://www.sciencedirect.com/science/article/pii/0925963596005468|see this paper]). After sonication the substrate is rinsed and blow-dried. | |||
Note that the substrate must be able to withstand high temperature (at least 700°C) and also high temperature gradients, as the center of the substrate is heated more than the edges. In practice this means that to grow diamond on Si it is necessary to use a thick Si substrate. Ordinary 500 micron thick 2" wafers break due to stress induced by the temperature gradient. | |||
Polishing is needed after deposition if the polycrystalline diamond layer has to be smooth. This cannot be done here at Nanolab, so the film must be sent away for polishing. Following polishing it is possible to etch the film in the metal ICP, but etching cannot take the place of polishing as different crystal faces of the diamond etch at different rates. | |||
Thinning is needed if the diamond layer has to be very thin as a uniform diamond layer can only be deposited above 1 μm thickness. | |||
<br clear="all" /> | <br clear="all" /> | ||
==Diamond formation (a bit of theory)== | ==Diamond formation (a bit of theory)== |
Revision as of 11:24, 19 October 2020
Feedback to this page: film deposition/DiamondCVD/Diamond_CVD_process_details click here
THIS PAGE IS UNDER CONSTRUCTION![Under construction.png](/images/thumb/f/f8/Under_construction.png/200px-Under_construction.png.jpeg)
Diamond growth by MPCVD at Nanolab
At Nanolab, it is possible to grow single- and polycrystalline diamond in the SEKI diamond CVD.
Single- and polycrystalline diamond
Single crystal diamond
It is possible to grow very clean diamond in the SEKI system. In theory it would even be possible to control the N2 dopant level and dopant depth. However, in practice it would be necessary to have our own hydrogen generator or to buy (very expensive) extra pure hydrogen to make this possible. The hydrogen we have for general processing at Nanolab simply contains too much nitrogen. To control doping levels it is necessary to use 7N hydrogen and to mix it with a very small additional flow of hydrogen mixed with only a few percent nitrogen.
Nitrogen doping affects the optical and electronic properties of the diamond. For instance this can be used in magnetic sensors, which is a topic of research at DTU Physics.
It is possible to grow single crystal diamond in the SEKI by using a single crystalline diamond substrate (these are purchased and typical dimensions might be 2x2 mm with 0.1 mm thickness). We have not investigated whether it is possible to distinguish the transition from the purchased substrate to the newly grown layer.
Polycrystalline diamond
For polycrystalline growth the substrate must be seeded with diamonds. This is commonly done by sonicating the substrate in a solution of water with nano diamonds, although other solvents may give better results (this paper). After sonication the substrate is rinsed and blow-dried.
Note that the substrate must be able to withstand high temperature (at least 700°C) and also high temperature gradients, as the center of the substrate is heated more than the edges. In practice this means that to grow diamond on Si it is necessary to use a thick Si substrate. Ordinary 500 micron thick 2" wafers break due to stress induced by the temperature gradient.
Polishing is needed after deposition if the polycrystalline diamond layer has to be smooth. This cannot be done here at Nanolab, so the film must be sent away for polishing. Following polishing it is possible to etch the film in the metal ICP, but etching cannot take the place of polishing as different crystal faces of the diamond etch at different rates.
Thinning is needed if the diamond layer has to be very thin as a uniform diamond layer can only be deposited above 1 μm thickness.
Diamond formation (a bit of theory)
Diamond is grown by depositing carbon from the CH4 on a substrate. If the carbon forms an sp3 bond to other carbon atoms, diamond is grown. Otherwise it will be etched away by a high concentration of H2. Diamond is very inert, but the plasma in the CVD equipment creates hydrogen radicals that in turn create active sites on the diamond surface. These active sites react with methane radicals that are also created in the plasma.