Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using AOE: Difference between revisions
Jump to navigation
Jump to search
No edit summary |
|||
Line 203: | Line 203: | ||
|- | |- | ||
|} | |} | ||
==Etching deep structures in quartz (micro size) with polySi as masking material== |
Revision as of 15:44, 31 July 2009
Danchip has recently (January 2009) taken over the AOE from Hymite. Not much process testing has been done yet.
Etching of micro structures in Silicon Oxide with photoresist or (poly)silicon as masking material
Parameter | Si mask | Resist mask |
---|---|---|
Coil Power [W] | 1300 | 1000 |
Platen Power [W] | 500 | 300 |
Platen temperature [oC] | 60 | 0 |
He flow [sccm] | 300 | 174 |
CF flow [sccm] | 18 | 10 |
H flow [sccm] | 0 | 8 |
Pressure [mTorr] | 4 | 4 |
Typical results | Si mask non-confirmed result | Si mask DANCHIP result | Resist mask non-confirmed result | Resist mask DANCHIP result |
---|---|---|---|---|
Etch rate [nm/min] | 500 | 460-480 (low aspect ratio) | 300 | 280, 300 |
Selectivity [:1] | 20 | ~15 | 4 | 3.2, 4 |
Profile [o] | >88 | 90.5-91.5 (negatively tapered) | >88 | ~88 |
Images | . | See here | . | See here |
Etching of micro structures in Silicon Oxide with Aluminium as masking material
Parameter | Al mask |
---|---|
Coil Power [W] | 1800 |
Platen Power [W] | 180 |
Platen temperature [oC] | 60 |
CF flow [sccm] | 80 |
O flow [sccm] | 10 |
Pressure [mTorr] | 6 |
Typical results | Al mask non-confirmed result | Al mask DANCHIP result |
---|---|---|
Etch rate [nm/min] | >500 | . |
Selectivity [:1] | >50 | . |
Profile [o] | >88 | . |
Etching of sub-micro structures (trenches or holes) in Silicon Oxide with (poly)silicon or Aluminium as masking material
Parameter | Si mask | Al mask | Very thin Al mask |
---|---|---|---|
Coil Power [W] | 1600 | 1100 | 2000 |
Platen Power [W] | 200 | 500 | 140 |
Platen temperature [oC] | 0 | 60 | 60 |
He flow [sccm] | 300 | 50 | 60 |
CF flow [sccm] | 6 | 26 | 29 |
H flow [sccm] | 18 | 0 | 0 |
O flow [sccm] | 0 | 0 | 16 |
Pressure [mTorr] | 4 | 8 | 3 |
Typical results | Si mask non-confirmed result | Si mask DANCHIP result | Al mask non-confirmed result | Al mask DANCHIP result | Thin Al mask non-confirmed result | Thin Al mask DANCHIP result |
---|---|---|---|---|---|---|
Etch rate [nm/min] | 200 | . | 275 | . | . | . |
Selectivity [:1] | 11 | . | >50 | . | Should be larger than for the other Al mask recipe | . |
Profile [o] | 86 | . | 90 | . | 90 | . |