Specific Process Knowledge/Thin film deposition/Deposition of Gold: Difference between revisions
Jump to navigation
Jump to search
No edit summary |
No edit summary |
||
Line 44: | Line 44: | ||
== Adhesion of Au on Si == | |||
[[/Adhesion of Au|Adhesion of Au layers]] | |||
== Studies of Au deposition processes == | == Studies of Au deposition processes == | ||
[[/Roughness of Au|Roughness of Au layers]] - ''Roughness of Au layers deposited with different equipment and settings'' | [[/Roughness of Au|Roughness of Au layers]] - ''Roughness of Au layers deposited with different equipment and settings'' |
Revision as of 13:47, 11 March 2009
Gold can be deposited by e-beam evaporation. In the chart below you can compare the different deposition equipment.
E-beam evaporation (Alcatel) | E-beam evaporation (Leybold) | E-beam evaporation (Wordentec) | Sputter (Lesker) | |
---|---|---|---|---|
Batch size |
|
|
|
|
Pre-clean | RF Ar clean | Ar ion bombartment | RF Ar clean | RF Ar clean |
Layer thickness | 10 Å to 1 µm | 10 Å to 1500 Å | 10 Å to 1 µm | 10 Å to |
Deposition rate | 2 Å/s to 15 Å/s | 1 Å/s to 5 Å/s | 1 Å/s to 15 Å/s |
Adhesion of Au on Si
Studies of Au deposition processes
Roughness of Au layers - Roughness of Au layers deposited with different equipment and settings