'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide/SiO2_etch_using_AOE/With_CSAR_resist_mask click here]''' | ||
''Information given by Alberto Cagliani February 2015'' | ''Information given by Alberto Cagliani February 2015'' | ||
Using the standard oxide recipe (SiO2_res) for 1 min the CSAR looked burned (test 2016-08-19 resist did not look burned after | Using the standard oxide recipe (SiO2_res) for 1 min the CSAR looked burned (test 2016-08-19 resist did not look burned after 1 min) and could not be removed by CSAR stripper (AR600-71). | ||
Using the following settings the resist did not looked burned and could be removed by CSAR stripper: | Using the following settings the resist did not looked burned and could be removed by CSAR stripper: | ||
Line 38: | Line 38: | ||
|-style="background:DarkGray; color:White" | |-style="background:DarkGray; color:White" | ||
!Typical results | !Typical results | ||
!Negative Resist mask | !Negative Resist mask Nanolab result | ||
|- | |- | ||
|Etch rate of thermal oxide | |Etch rate of thermal oxide |
Revision as of 22:44, 25 November 2019
Feedback to this page: click here
Information given by Alberto Cagliani February 2015
Using the standard oxide recipe (SiO2_res) for 1 min the CSAR looked burned (test 2016-08-19 resist did not look burned after 1 min) and could not be removed by CSAR stripper (AR600-71). Using the following settings the resist did not looked burned and could be removed by CSAR stripper:
Parameter | Recipe name: |
---|---|
Coil Power [W] | 450 |
Platen Power [W] | 80 |
Platen temperature [oC] | 0 |
He flow [sccm] | 174 |
C4F8 flow [sccm] | 5 |
H2 flow [sccm] | 4 |
Pressure [mTorr] | 4 |
Typical results | Negative Resist mask Nanolab result |
---|---|
Etch rate of thermal oxide | ~105nm/min (<5% etch load) |
Selectivity to CSAR [:1] | ~2 |
Profile [o] | not measured |
Images | none |
Comments | CSAR did not burn and could be removed by AR600-71 |