Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using RIE1 or RIE2: Difference between revisions
No edit summary |
No edit summary |
||
Line 167: | Line 167: | ||
{| border="0" cellspacing="1" cellpadding="3" align="left" | {| border="0" cellspacing="1" cellpadding="3" align="left" | ||
! | ! | ||
'''The Design of the experiment''' | |||
{| border="1" cellspacing="1" cellpadding="2" align="left" | {| border="1" cellspacing="1" cellpadding="2" align="left" | ||
! Recipe: | ! Recipe: | ||
Line 186: | Line 186: | ||
|} | |} | ||
! | ! | ||
'''Etch rate''' | |||
{| border="2" cellspacing="1" cellpadding="3" align="right" | {| border="2" cellspacing="1" cellpadding="3" align="right" | ||
![[image:RIE1_SIO2_DOE1_Etch_rate.jpg|300x300px|thumb|left|Etch rate as a function of power and pressure at 70% CHF<sub>3</sub>. The etch rate decreases a little as a function of %CHF<sub>3</sub>. ]] | ![[image:RIE1_SIO2_DOE1_Etch_rate.jpg|300x300px|thumb|left|Etch rate as a function of power and pressure at 70% CHF<sub>3</sub>. The etch rate decreases a little as a function of %CHF<sub>3</sub>. ]] | ||
Line 194: | Line 194: | ||
|} | |} | ||
<br /> | <br clear="all" /> | ||
'''Selectivity to photoresist''' | |||
{| border="0" cellspacing="1" cellpadding="3" align="Left" | {| border="0" cellspacing="1" cellpadding="3" align="Left" | ||
! | ! | ||
{| border="2" cellspacing="1" cellpadding="3" align="Left" | {| border="2" cellspacing="1" cellpadding="3" align="Left" | ||
![[image:RIE1_SIO2_DOE1_Selectivitet_65.jpg|250x200px|thumb|Left|Selectivity as a function of power and pressure at 65% CHF<sub>3</sub>. ]] | ![[image:RIE1_SIO2_DOE1_Selectivitet_65.jpg|250x200px|thumb|Left|Selectivity as a function of power and pressure at 65% CHF<sub>3</sub>. ]] |
Revision as of 10:24, 26 November 2008
RIE (Reactive Ion Etch) can be used for etching silicon oxide. The etch is anisotropic with vertical or angled sidewalls depending on the process recipe and the masking material and geometry. The SiO2 is etched by flour radicals assisted by ion bombardment.
The substrate:
Most be a wafer of 4" or below or small pieces, not higher than about 2mm.
The silicon can be masked by these materials:
- Photoresist
- E-beam resist
- Silicon
- Silicon Nitride
- Aluminium
- Chromium (ONLY RIE2!)
- Other metals if they cover less than 5% of the wafer area (ONLY RIE2!)
Most used recipes:
Resist as masking material:
Recipe: | 1SiO2mre |
---|---|
Masking material | Photoresist |
CF4 flow | 14 sccm |
CHF3 flow | 26 sccm |
Pressure | 100 mTorr |
RF-power | 60 W |
Expected results in RIE1 | Expected results in RIE2 | |
---|---|---|
Etch rate in SiO2 | ~20-30 nm/min | ~20-30 nm/min |
Etch rate in Si3N4 | ? | ? |
Etch rate in P-Si (when used as mask) | ~30 nm/min | ~30 nm/min |
Etch rate in Si
(etching down to Si) |
Expected <2 nm/min | Expected <2 nm/min |
mre:mask resist
PolySilicon as masking material
Recipe: | 1SiO2msi |
---|---|
Masking material | Silicon |
CF4 flow | 8 sccm |
CHF3 flow | 40 sccm |
Pressure | 150 mTorr |
RF-power | 150 W |
Expected results in RIE1 | Expected results in RIE2 | |
---|---|---|
Etch rate in SiO2 | ~70-80 nm/min | ~70-80 nm/min |
Etch rate in Si3N4 | ? | ? |
Etch rate in P-Si (when used as mask) | ~20-30 nm/min | ~20-30 nm/min |
Etch rate in Si
(etching down to Si) |
? | ? |
msi:mask silicon
Burned resist as masking material (developed for waveguides by Haiyan Ou @DTU Photonics):
Recipe: | 1SiO2mbr |
---|---|
Masking material | Burned resist (250oC) |
CHF3 flow | 84 sccm |
Pressure | 60 mTorr |
RF-power | 200 W |
Expected results in RIE1 | Expected results in RIE2 | |
---|---|---|
Etch rate in SiO2 | ~120 nm/min | ~120 nm/min |
Etch rate burned resist | ? | ? |
Etch rate in Si3N4 | ? | ? |
Etch rate in P-Si (when used as mask) | ? nm/min | ? nm/min |
Etch rate in Si
(etching down to Si) |
? | ? |
mbr:mask burned resist
A survey of the parameter space using photoresist as masking material
A DOE has been performed. A short summery is given here: (in progress)
RIE1:
A Design Of Experiment (DOE) has been performed. A screening experiment: full factorial with to levels: 9 different runs and 3 repetitions. Results from a screening experiment should be taken "with a gain of salt" meaning use it only as a rough guide line and test your recipe before use.
The Design of the experiment
|
Etch rate |
---|
Selectivity to photoresist
|
---|
More details on the DOE can be seen here: "DOE RIE1 siliconoxide etch of small structures" (not available yet).