Specific Process Knowledge/Etch/Aluminum Oxide/Al2O3 Etch with ICP Metal: Difference between revisions
No edit summary |
No edit summary |
||
Line 4: | Line 4: | ||
|-style="background:Black; color:White" | |-style="background:Black; color:White" | ||
! Parameter | ! Parameter | ||
|Recipe name: '''no name | |Recipe name: '''no name''' (testing recipe) | ||
|- | |- | ||
|Coil Power [W] | |Coil Power [W] | ||
Line 34: | Line 34: | ||
|Al2O3 | |Al2O3 | ||
| | | | ||
*'''~93nm/min (30s, 1/4 wafer on 6" carrier)'''<br> ''2017-01-20 bghe@ | *'''~93nm/min (30s, 1/4 wafer on 6" carrier)'''<br> ''2017-01-20 bghe@nanolab'' | ||
|- | |- | ||
Revision as of 11:08, 28 January 2019
Feedback to this page: click here
Parameter | Recipe name: no name (testing recipe) |
---|---|
Coil Power [W] | 1200 |
Platen Power [W] | 200 |
Platen temperature [oC] | 0 |
BCl3 flow [sccm] | 60 |
Cl2 flow [sccm] | 30 |
Pressure [mTorr] | 4 |
Material to be etched | Etch rate using the above parameters |
---|---|
Al2O3 |
|