Specific Process Knowledge/Thin film deposition/Deposition of Gold: Difference between revisions
(→Adhesion of Au on Si: Added Temescal. Various small tweaks) |
|||
Line 9: | Line 9: | ||
*[[/Adhesion layers|Adhesion layers]] | *[[/Adhesion layers|Adhesion layers]] | ||
== Au deposition == | |||
Below you can compare the different equipment that allows Au deposition. | |||
{| border="1" cellspacing="0" cellpadding="4" | {| border="1" cellspacing="0" cellpadding="4" | ||
Line 14: | Line 17: | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" | ||
! | ! | ||
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/ | ! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|E-beam evaporator Temescal]]) | ||
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]]) | ! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]]) | ||
! Sputter ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]]) | ! Sputter ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]]) | ||
Line 31: | Line 34: | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! Pre-clean | ! Pre-clean | ||
| | |Ar ion source | ||
|RF Ar clean | |RF Ar clean | ||
|RF Ar clean | |RF Ar clean | ||
Line 40: | Line 43: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! Layer thickness | ! Layer thickness | ||
|10 Å to | |10 Å to 1 µm* | ||
|10 Å to | |10 Å to 5000 Å* | ||
|10 Å to | |10 Å to | ||
| | |10 Å to about 3000 Å** | ||
| | | | ||
| | | | ||
Line 50: | Line 53: | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! Deposition rate | ! Deposition rate | ||
| | |0.5 Å/s to 10 Å/s | ||
|1 Å/s to 10 Å/s | |1 Å/s to 10 Å/s | ||
| | | | ||
Line 62: | Line 65: | ||
! Batch size | ! Batch size | ||
| | | | ||
*Up to | *Up to 4x6" wafers or | ||
*smaller pieces | *Up to 3x8" wafers (ask for special holder) | ||
*many smaller pieces | |||
| | | | ||
*24x2" wafers or | *24x2" wafers or | ||
Line 89: | Line 93: | ||
| | | | ||
* Silicon oxide | *Silicon | ||
* Silicon (oxy)nitride | *Silicon oxide | ||
* Photoresist | *Silicon (oxy)nitride | ||
* PMMA | *Photoresist | ||
* Mylar | *PMMA | ||
* | *Mylar | ||
* | *Metals | ||
*See also the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet] | |||
| | | | ||
* Silicon oxide | * Silicon oxide | ||
Line 128: | Line 133: | ||
! Comment | ! Comment | ||
| | | | ||
* For thicknesses above | * For thicknesses above 600 nm permission is required | ||
* An adhesion layer (of Cr or Ti) is recommended under Au. | * An adhesion layer (of Cr or Ti) is recommended under Au. | ||
* Takes approx. 20 min to pump down. | |||
| | | | ||
* For thicknesses above | * For thicknesses above 600 nm permission is required | ||
* An adhesion layer (of Cr or Ti) is recommended under Au. | * An adhesion layer (of Cr or Ti) is recommended under Au. | ||
* Takes approx. 1 hour to pump down. | |||
| | | | ||
| | | | ||
* For thicknesses above 200 nm permission is required | |||
* An adhesion layer (of Cr or Ti) is recommended under Au. | |||
| | | | ||
* Used for gold sputter coating of samples before SEM inspection | * Used for gold sputter coating of samples before SEM inspection | ||
* Very fast. | |||
| | | | ||
* Used for gold sputter coating of samples before SEM inspection | * Used for gold sputter coating of samples before SEM inspection | ||
*Very fast. | |||
|- | |- | ||
|} | |} | ||
'''*''' ''For thicknesses above 200 nm | '''*''' ''For thicknesses above 600 nm write to metal@danchip.dtu.dk to ensure that there will be enough material in the machine.'' | ||
'''**''' ''For thicknesses above 200 nm write to metal@danchip.dtu.dk to ensure that there will be enough material in the machine.'' | |||
== Studies of Au deposition processes in the Wordentec== | == Studies of Au deposition processes in the Wordentec== |
Revision as of 11:46, 30 July 2018
Feedback to this page: click here
Gold can be deposited by e-beam evaporation or sputtering. In the chart below you can compare the different deposition equipment.
Adhesion of Au on Si
The adhesion of gold on Silicon or Silicon with native oxide is not very good. The Si substrate is often deposited an adhesion layer before the gold deposition. A few nm of Chromium or Titanium works well and they react with the Oxygen of Silicon oxide and present a metallic bond with gold. 5 nm to 10 nm thick of Cr or Ti is commonly used and it is important to deposit Cr or Ti and then immediately Au. If the vacuum chamber is opened in between, the surface of Cr or Ti will get oxidized and that will give a poor adhesion. If a gold layer needs to be deposited directly on Silicon, then native oxide has to be removed by deep in diluted HF and immediately load the evaporation chamber. And after the deposition, the wafer has to be heated op to get some Au-Si diffusion which improves the adhesion.
Au deposition
Below you can compare the different equipment that allows Au deposition.
E-beam evaporation (E-beam evaporator Temescal) | E-beam evaporation (Wordentec) | Sputter (Lesker) | E-beam evaporation (Physimeca) | Sputter coater (Sputter coater 03) | Sputter coater (Sputter coater 04) | |
---|---|---|---|---|---|---|
General description | E-beam deposition of Au | E-beam deposition of Au | Sputter deposition of Au | E-beam deposition of Au | Sputter deposition of Au | Sputter deposition of Au |
Pre-clean | Ar ion source | RF Ar clean | RF Ar clean | |||
Layer thickness | 10 Å to 1 µm* | 10 Å to 5000 Å* | 10 Å to | 10 Å to about 3000 Å** | ||
Deposition rate | 0.5 Å/s to 10 Å/s | 1 Å/s to 10 Å/s | From 5 Å/s up to 10Å/s | Not measured | Not measured | |
Batch size |
|
|
|
|
|
|
Allowed materials |
|
|
|
|
|
|
Comment |
|
|
|
|
|
* For thicknesses above 600 nm write to metal@danchip.dtu.dk to ensure that there will be enough material in the machine.
** For thicknesses above 200 nm write to metal@danchip.dtu.dk to ensure that there will be enough material in the machine.
Studies of Au deposition processes in the Wordentec
Roughness of Au layers - Roughness of Au layers deposited with different equipment and settings
Wafer temperature
The wafer temperature during e-beam deposition of 200 nm Au on six wafers has been measured using thermal labels on the backside of the wafers. The following results were obtained:
Wafer | Temperature [C] |
---|---|
1 | 48 |
2 | 60 |
3 | 65 |
4 | 71 |
5 | 71 |
6 | 77 |
The temperatures are accurate within approximately +/- 3C and probably underestimating the actual wafer temperature slightly. It is observed that the wafer temperature increases with each wafer, thus if wafer temperature is of concern it is advised to reduce the number of wafers per run.
Thin Au layer deposition using Lesker
For depositing very thin, down to 6nm continuous Au layers on Si/SiO2 substrates. Works also with ALD deposited Al2O3 and TiO2 as substrate.
Adhesion promoter: aminopropyltrimethoxysilane (APTMS). MSDS here.
Adhesion promoter deposition: 3h immersion in 95%IPA, 2.5% H2O, 2.5% APTMS.
NOTE: the APTMS layer is degrading quickly in atmosphere, so deposit it as close to the Au deposition as possible.
Lesker deposition parameters:
Gun # | Power [W] | Ramp rate [W/s] | Pressure [mtorr] | Atmosphere | Deposition rate [nm/s] |
---|---|---|---|---|---|
2 | 300 | 5 | 3 | Ar | 1 |
NOTE: As a general rule, the lower the pressure and higher the power (i.e. higher the deposition rate), the better.
Film characteristics (5-10 wafers for each thickness):
Thickness [nm] | Roughness min [nm] | Roughness max [nm] |
---|---|---|
6 | 0.25 | 0.4 |
10 | 0.3 | 0.5 |
24 | 0.3 | 0.5 |
NOTE: After depositing 10 layers of 10nm each, one on top of each other, the roughness increased to 0.8nm RMS
Work done by Johneph Sukham (@ DTU Fotonik) and Radu Malureanu (@ DTU Fotonik and DTU Danchip) in 2016-2017.