Specific Process Knowledge/Thin film deposition/ALD Picosun R200/ZnO deposition using ALD: Difference between revisions
Line 50: | Line 50: | ||
image:ALD_growth_rate_ZnO.jpg|Figure 1. a) Linear growth (~0.15 nm/cycles) @ 200 <sup>o</sup>C. b) ALD-window for ZnO deposition. | image:ALD_growth_rate_ZnO.jpg|Figure 1. a) Linear growth (~0.15 nm/cycles) @ 200 <sup>o</sup>C. b) ALD-window for ZnO deposition. | ||
image:ALD_SE_ZnO.jpg|Figure 2. a) Typical uniformity profile across 100mm Si wafer based on 49 mesurement points. b) Photography of the prepared wafer. | image:ALD_SE_ZnO.jpg|Figure 2. a) Typical uniformity profile across 100mm Si wafer based on 49 mesurement points. b) Photography of the prepared wafer. | ||
</gallery> | |||
<br clear="all" /> | |||
<b>Evgeniy Shkondin, DTU Danchip, 2014-2016.</b> | |||
<br clear="all" /> | |||
<br clear="all" /> | |||
===ZnO XPS investigation for elemental trace analysis and deposition on high aspect ratio structures=== | |||
XPS profile for ZnO has been obtained using [[Specific_Process_Knowledge/Characterization/XPS#XPS-ThermoScientific|XPS-ThermoScientific]]. ZnO samples reveals (see Figure 3a) chemically high quality films with no observable contaminations in temperature range 100 - 250 <sup>o</sup>C. | |||
The recipe is good for deposition on very high aspect ratio structures (with aspect ratio more than 1:20) such as deep trenches, pillars, pores etc. <b>ZnOT</b> can also be used for deposition on polymers at low temperatures (80-120 <sup>o</sup>C). | |||
<!--Research results based on this recipe can be found here: [http://scitation.aip.org/content/avs/journal/jvsta/34/3/10.1116/1.4947586 LINK] (J. Vac. Sci. Technol. A 34(3), 2016 031605)--> | |||
<gallery caption="" widths="700px" heights="300px" perrow="2"> | |||
image:ALD_SEM_ZnO_trenches_ALD.jpg|Figure 3. a) XPS survey scan b) SEM images of ZnO deposited on a Si trenches at 200 <sup>o</sup>C temperature and 700 cycles. Trenches prepered using [[Specific_Process_Knowledge/Etch/DRIE-Pegasus|DRIE-Pegasus]]. Inset image shows the photography of the sample. | |||
</gallery> | </gallery> | ||
Revision as of 11:11, 20 March 2017
The ALD window for deposition of zinc oxide (ZnO) ranges from 100 oC to 250 oC. Several investigation techniques has been implemented for ZnO characterization. Additionally, more information on ZnO can be found on a page about Al-doped ZnO (AZO)
All results shown on this page have been obtained using the "ZnOT" recipe on new Si(100) wafers with native oxide:
ZnO standard recipe
Recipe: ZnOT
Maximum deposition thickness: 100 nm
Temperature: 100 oC - 250 oC
DEZ* | DEZ | H2O | H2O | |
---|---|---|---|---|
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
DEZ is diethylzinc (Zn(CH2CH3)2 or ZnEt2)
ZnO deposition rates and uniformity
The deposition rate for ZnO depends on the temperature, see the ALD-window graph below. The uniformity, thickness, refractive index has been obtained using Ellipsometer VASE.
Evgeniy Shkondin, DTU Danchip, 2014-2016.
ZnO XPS investigation for elemental trace analysis and deposition on high aspect ratio structures
XPS profile for ZnO has been obtained using XPS-ThermoScientific. ZnO samples reveals (see Figure 3a) chemically high quality films with no observable contaminations in temperature range 100 - 250 oC.
The recipe is good for deposition on very high aspect ratio structures (with aspect ratio more than 1:20) such as deep trenches, pillars, pores etc. ZnOT can also be used for deposition on polymers at low temperatures (80-120 oC).
Figure 3. a) XPS survey scan b) SEM images of ZnO deposited on a Si trenches at 200 oC temperature and 700 cycles. Trenches prepered using DRIE-Pegasus. Inset image shows the photography of the sample.