Specific Process Knowledge/Thin film deposition/ALD Picosun R200/AZO deposition using ALD: Difference between revisions
Line 4: | Line 4: | ||
AZO can be deposited in a temperature window 150 - 250 <sup>o</sup>C. Physical and optical properties are strongly corelated with deposition temperture and Al doping concentration. | AZO can be deposited in a temperature window 150 - 250 <sup>o</sup>C. Physical and optical properties are strongly corelated with deposition temperture and Al doping concentration. | ||
All results shown on this page have been obtained using the Si(100) wafers with native oxide as substrates: | All results shown on this page have been obtained using the Si(100) wafers with native oxide as substrates: | ||
==Al-doped ZnO (AZO) standard recipes== | |||
<b>Recipe: AZO 20T</b> | |||
<b>Maximum deposition thickness: 100 nm</b> | |||
<b>Temperature: 150 <sup>o</sup>C - 250 <sup>o</sup>C</b> | |||
{| border="2" cellspacing="2" cellpadding="9" align="none" | |||
|- | |||
!# macrocycles | |||
|colspan="8" align="center"|<i>n</i> | |||
|- | |||
!# cycles | |||
|colspan="4" align="center"|19 | |||
|colspan="4" align="center"|1 | |||
|- | |||
!Precursor | |||
!DEZ | |||
!DEZ | |||
!H<sub>2</sub>O | |||
!H<sub>2</sub>O | |||
!TMA | |||
!TMA | |||
!H<sub>2</sub>O | |||
!H<sub>2</sub>O | |||
|- | |||
!Nitrogen flow | |||
|150 sccm | |||
|150 sccm | |||
|200 sccm | |||
|200 sccm | |||
|150 sccm | |||
|150 sccm | |||
|200 sccm | |||
|200 sccm | |||
|- | |||
!Pulse time | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|- | |||
!Purge time | |||
|0.5 s | |||
|20.0 s | |||
|0.5 s | |||
|20.0 s | |||
|0.5 s | |||
|20.0 s | |||
|0.5 s | |||
|20.0 s | |||
|- | |||
|} | |||
<b>How to fill out the process log in LabManager:</b> | |||
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle. | |||
<strong>DEZ</strong> pulse time: (0.1 + 0.1) s * 19 = <strong>3.8 s</strong> | |||
<strong>TMA</strong> pulse time: (0.1 + 0.1 )s * 1 = <strong>0.2 s</strong> | |||
<strong>H<sub>2</sub>O</strong> pulse time: [(0.1 + 0.1) s * 19] + [(0.1 + 0.1) s * 1] = <strong>4.0 s</strong> | |||
The number of cycles for each precursor now equals the number of macrocycles (<i>n</i>). | |||
<b>Recipe: AZO 25T</b> | |||
<b>Maximum deposition thickness: 100 nm</b> | |||
<b>Temperature: 150 <sup>o</sup>C - 250 <sup>o</sup>C</b> | |||
{| border="2" cellspacing="2" cellpadding="9" align="none" | |||
|- | |||
!# macrocycles | |||
|colspan="8" align="center"|<i>n</i> | |||
|- | |||
!# cycles | |||
|colspan="4" align="center"|24 | |||
|colspan="4" align="center"|1 | |||
|- | |||
!Precursor | |||
!DEZ | |||
!DEZ | |||
!H<sub>2</sub>O | |||
!H<sub>2</sub>O | |||
!TMA | |||
!TMA | |||
!H<sub>2</sub>O | |||
!H<sub>2</sub>O | |||
|- | |||
!Nitrogen flow | |||
|150 sccm | |||
|150 sccm | |||
|200 sccm | |||
|200 sccm | |||
|150 sccm | |||
|150 sccm | |||
|200 sccm | |||
|200 sccm | |||
|- | |||
!Pulse time | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|- | |||
!Purge time | |||
|0.5 s | |||
|20.0 s | |||
|0.5 s | |||
|20.0 s | |||
|0.5 s | |||
|20.0 s | |||
|0.5 s | |||
|20.0 s | |||
|- | |||
|} | |||
<b>How to fill out the process log in LabManager:</b> | |||
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle. | |||
<strong>DEZ</strong> pulse time: (0.1 + 0.1) s * 24 = <strong>4.8 s</strong> | |||
<strong>TMA</strong> pulse time: (0.1 + 0.1 )s * 1 = <strong>0.2 s</strong> | |||
<strong>H<sub>2</sub>O</strong> pulse time: [(0.1 + 0.1) s * 24] + [(0.1 + 0.1) s * 1] = <strong>5.0 s</strong> | |||
The number of cycles for each precursor now equals the number of macrocycles (<i>n</i>). | |||
<b>Recipe: AZO 30T</b> | |||
<b>Maximum deposition thickness: 100 nm</b> | |||
<b>Temperature: 150 <sup>o</sup>C - 250 <sup>o</sup>C</b> | |||
{| border="2" cellspacing="2" cellpadding="9" align="none" | |||
|- | |||
!# macrocycles | |||
|colspan="8" align="center"|<i>n</i> | |||
|- | |||
!# cycles | |||
|colspan="4" align="center"|29 | |||
|colspan="4" align="center"|1 | |||
|- | |||
!Precursor | |||
!DEZ | |||
!DEZ | |||
!H<sub>2</sub>O | |||
!H<sub>2</sub>O | |||
!TMA | |||
!TMA | |||
!H<sub>2</sub>O | |||
!H<sub>2</sub>O | |||
|- | |||
!Nitrogen flow | |||
|150 sccm | |||
|150 sccm | |||
|200 sccm | |||
|200 sccm | |||
|150 sccm | |||
|150 sccm | |||
|200 sccm | |||
|200 sccm | |||
|- | |||
!Pulse time | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|- | |||
!Purge time | |||
|0.5 s | |||
|20.0 s | |||
|0.5 s | |||
|20.0 s | |||
|0.5 s | |||
|20.0 s | |||
|0.5 s | |||
|20.0 s | |||
|- | |||
|} | |||
<b>How to fill out the process log in LabManager:</b> | |||
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle. | |||
<strong>DEZ</strong> pulse time: (0.1 + 0.1) s * 29 = <strong>5.8 s</strong> | |||
<strong>TMA</strong> pulse time: (0.1 + 0.1 )s * 1 = <strong>0.2 s</strong> | |||
<strong>H<sub>2</sub>O</strong> pulse time: [(0.1 + 0.1) s * 29] + [(0.1 + 0.1) s * 1] = <strong>6.0 s</strong> | |||
The number of cycles for each precursor now equals the number of macrocycles (<i>n</i>). | |||
<b>Recipe: AZO 35T</b> | |||
<b>Maximum deposition thickness: 100 nm</b> | |||
<b>Temperature: 150 <sup>o</sup>C - 250 <sup>o</sup>C</b> | |||
{| border="2" cellspacing="2" cellpadding="9" align="none" | |||
|- | |||
!# macrocycles | |||
|colspan="8" align="center"|<i>n</i> | |||
|- | |||
!# cycles | |||
|colspan="4" align="center"|34 | |||
|colspan="4" align="center"|1 | |||
|- | |||
!Precursor | |||
!DEZ | |||
!DEZ | |||
!H<sub>2</sub>O | |||
!H<sub>2</sub>O | |||
!TMA | |||
!TMA | |||
!H<sub>2</sub>O | |||
!H<sub>2</sub>O | |||
|- | |||
!Nitrogen flow | |||
|150 sccm | |||
|150 sccm | |||
|200 sccm | |||
|200 sccm | |||
|150 sccm | |||
|150 sccm | |||
|200 sccm | |||
|200 sccm | |||
|- | |||
!Pulse time | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|0.1 s | |||
|- | |||
!Purge time | |||
|0.5 s | |||
|20.0 s | |||
|0.5 s | |||
|20.0 s | |||
|0.5 s | |||
|20.0 s | |||
|0.5 s | |||
|20.0 s | |||
|- | |||
|} | |||
<b>How to fill out the process log in LabManager:</b> | |||
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle. | |||
<strong>DEZ</strong> pulse time: (0.1 + 0.1) s * 34 = <strong>6.8 s</strong> | |||
<strong>TMA</strong> pulse time: (0.1 + 0.1 )s * 1 = <strong>0.2 s</strong> | |||
<strong>H<sub>2</sub>O</strong> pulse time: [(0.1 + 0.1) s * 34] + [(0.1 + 0.1) s * 1] = <strong>7.0 s</strong> | |||
The number of cycles for each precursor now equals the number of macrocycles (<i>n</i>). | |||
===AZO deposition rates=== | |||
The deposition rate for AZO depends on the temperature, see the ALD-window graph below. The uniformity, thickness, refractive index has been obtained using [[Specific_Process_Knowledge/Characterization/Optical_characterization#Ellipsometer|Ellipsometer VASE]]. | |||
<gallery caption="" widths="600px" heights="400px" perrow="3"> | |||
image:AZO_recipe_overview_eves16032017.jpg| ALD-window for Al<sub>2</sub>O<sub>3</sub> deposition. | |||
image:AZO_deposition_overview_eves16032017.jpg| Typical uniformity profile across 100mm Si wafer based on 49 mesurement points. | |||
image:AZO_growth_rate_eves16032017.jpg| Typical uniformity profile across 100mm Si wafer based on 49 mesurement points. | |||
</gallery> | |||
In the graphs below the Al<sub>2</sub>O<sub>3</sub> thickness as function of number of cycles for deposition temperatures between 100 <sup>o</sup>C and 350 <sup>o</sup>C can be seen. From the equations the number of cycles required for a certain thickess can be calculated. | |||
==Al-doped ZnO (AZO) standard recipes== | ==Al-doped ZnO (AZO) standard recipes== | ||
Revision as of 18:44, 16 March 2017
AZO can be deposited in a temperature window 150 - 250 oC. Physical and optical properties are strongly corelated with deposition temperture and Al doping concentration. All results shown on this page have been obtained using the Si(100) wafers with native oxide as substrates:
Al-doped ZnO (AZO) standard recipes
Recipe: AZO 20T
Maximum deposition thickness: 100 nm
Temperature: 150 oC - 250 oC
# macrocycles | n | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 19 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 19 = 3.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 19] + [(0.1 + 0.1) s * 1] = 4.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
Recipe: AZO 25T
Maximum deposition thickness: 100 nm
Temperature: 150 oC - 250 oC
# macrocycles | n | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 24 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 24 = 4.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 24] + [(0.1 + 0.1) s * 1] = 5.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
Recipe: AZO 30T
Maximum deposition thickness: 100 nm
Temperature: 150 oC - 250 oC
# macrocycles | n | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 29 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 29 = 5.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 29] + [(0.1 + 0.1) s * 1] = 6.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
Recipe: AZO 35T
Maximum deposition thickness: 100 nm
Temperature: 150 oC - 250 oC
# macrocycles | n | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 34 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 34 = 6.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 34] + [(0.1 + 0.1) s * 1] = 7.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
AZO deposition rates
The deposition rate for AZO depends on the temperature, see the ALD-window graph below. The uniformity, thickness, refractive index has been obtained using Ellipsometer VASE.
In the graphs below the Al2O3 thickness as function of number of cycles for deposition temperatures between 100 oC and 350 oC can be seen. From the equations the number of cycles required for a certain thickess can be calculated.
Al-doped ZnO (AZO) standard recipes
Recipe: AZO 20T
Maximum deposition thickness: 100 nm
Temperature: 150 oC - 250 oC
# macrocycles | n | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 19 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 19 = 3.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 19] + [(0.1 + 0.1) s * 1] = 4.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
Recipe: AZO 25T
Maximum deposition thickness: 100 nm
Temperature: 150 oC - 250 oC
# macrocycles | n | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 24 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 24 = 4.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 24] + [(0.1 + 0.1) s * 1] = 5.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
Recipe: AZO 30T
Maximum deposition thickness: 100 nm
Temperature: 150 oC - 250 oC
# macrocycles | n | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 29 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 29 = 5.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 29] + [(0.1 + 0.1) s * 1] = 6.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
Recipe: AZO 35T
Maximum deposition thickness: 100 nm
Temperature: 150 oC - 250 oC
# macrocycles | n | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 34 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 34 = 6.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 34] + [(0.1 + 0.1) s * 1] = 7.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
AZO deposition rates
The deposition rate for AZO depends on the temperature, see the ALD-window graph below. The uniformity, thickness, refractive index has been obtained using Ellipsometer VASE.
In the graphs below the Al2O3 thickness as function of number of cycles for deposition temperatures between 100 oC and 350 oC can be seen. From the equations the number of cycles required for a certain thickess can be calculated.