*'''~ | *'''~93nm/min (30s, 1/4 wafer on 6" carrier)'''<br> ''2017-01-20 bghe@danchip'' | ||
|- | |- | ||
Revision as of 15:08, 20 January 2017
Feedback to this page: click here
THIS PAGE IS UNDER CONSTRUCTION
Parameter | Recipe name: no name yet (testing recipe) |
---|---|
Coil Power [W] | 1200 |
Platen Power [W] | 200 |
Platen temperature [oC] | 0 |
BCl3 flow [sccm] | 60 |
Cl2 flow [sccm] | 30 |
Pressure [mTorr] | 4 |
Etch rates in different materials using the standard "Silicon oxide etch with resist mask"
Material to be etched | Etch rate using the above parameters |
---|---|
Al2O3 |
|