Specific Process Knowledge/Etch/DRIE-Pegasus/processA/PrA-2: Difference between revisions
< Specific Process Knowledge | Etch | DRIE-Pegasus | processA
Jump to navigation
Jump to search
No edit summary |
No edit summary |
||
Line 7: | Line 7: | ||
! colspan="2" width="120"| Substrate Information | ! colspan="2" width="120"| Substrate Information | ||
! colspan="3" | Process Information | ! colspan="3" | Process Information | ||
! rowspan="2 | ! rowspan="2" |SEM Images | ||
|- | |- | ||
! width="30" | Wafer info | ! width="30" | Wafer info |
Revision as of 12:45, 22 June 2016
Date | Substrate Information | Process Information | SEM Images | |||
---|---|---|---|---|---|---|
Wafer info | Exposed area | Conditioning | Recipe | Wafer ID | ||
2/5-2016 | 4" Travka20 Wafer | 20 % Si | 3 minute TDESC clean | PrA-2, 80 cycles or 14:40 minutes | C03991.03 | |
2/5-2016 | 4" Travka20 Wafer | 20 % Si | 3 minute TDESC clean | PrA-2, 80 cycles or 14:40 minutes | C03991.06 | |
3/6-2016 | 4" Travka20 Wafer | 20 % Si | 3 minute TDESC clean | PrA-2, 80 cycles or 14:40 minutes | C04047.03 | |
3/6-2016 | 4" Travka20 Wafer | 20 % Si | 3 minute TDESC clean | PrA-2, 80 cycles or 14:40 minutes | C04047.06 |