'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/III-V_ICP/SiO2 click here]''' | '''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/III-V_ICP/SiO2 click here]''' | ||
{| border="2" cellspacing="2" cellpadding="3" | {| border="2" cellspacing="2" cellpadding="3" |
Revision as of 11:09, 11 February 2016
Feedback to this page: click here
Parameter | Resist mask |
---|---|
Coil Power [W] | 200 |
Platen Power [W] | 25 |
Platen temperature [oC] | 0 |
CF4 flow [sccm] | 20 |
H2 flow [sccm] | 10 |
Pressure [mTorr] | 3 |
Results | Test by Artem Shikin @ Fotonik |
---|---|
Etch rate of PECVD BPSG | 39.4nm/min (22-01-2016) |
Selectivity to resist [:1] | Not known |
Wafer uniformity (100mm) | Not known |
Profile [o] | Not known |
Wafer uniformity map (click on the image to view a larger image) | Not known |
SEM profile images | NONE |
Comment | Tested on a plane BPSG layer. The etch rate is much lower for an etch time of e.g. 5s |