Specific Process Knowledge/Etch/III-V ICP/SiO2: Difference between revisions
No edit summary |
|||
Line 54: | Line 54: | ||
|- | |- | ||
|Comment | |Comment | ||
| | |Tested on a plane BPSG layer. The etch rate is much lower for an etch time of e.g. 5s | ||
|- | |- | ||
|} | |} |
Revision as of 11:09, 11 February 2016
Feedback to this page: click here
THIS PAGE IS UNDER CONSTRUCTION
Parameter | Resist mask |
---|---|
Coil Power [W] | 200 |
Platen Power [W] | 25 |
Platen temperature [oC] | 0 |
CF4 flow [sccm] | 20 |
H2 flow [sccm] | 10 |
Pressure [mTorr] | 3 |
Results | Test by Artem Shikin @ Fotonik |
---|---|
Etch rate of PECVD BPSG | 39.4nm/min (22-01-2016) |
Selectivity to resist [:1] | Not known |
Wafer uniformity (100mm) | Not known |
Profile [o] | Not known |
Wafer uniformity map (click on the image to view a larger image) | Not known |
SEM profile images | NONE |
Comment | Tested on a plane BPSG layer. The etch rate is much lower for an etch time of e.g. 5s |