Specific Process Knowledge/Etch/III-V ICP/SiO2: Difference between revisions
No edit summary |
|||
Line 15: | Line 15: | ||
|- | |- | ||
|Platen temperature [<sup>o</sup>C] | |Platen temperature [<sup>o</sup>C] | ||
| | |20 | ||
|- | |- | ||
|CF<sub>4</sub> flow [sccm] | |CF<sub>4</sub> flow [sccm] |
Revision as of 10:47, 11 February 2016
Feedback to this page: click here
THIS PAGE IS UNDER CONSTRUCTION
Parameter | Resist mask |
---|---|
Coil Power [W] | 800 |
Platen Power [W] | 100 |
Platen temperature [oC] | 20 |
CF4 flow [sccm] | 30 |
H2 flow [sccm] | 10 |
Pressure [mTorr] | 4 |
Results | Test on wafer with 50% load (Travka 50), by BGHE @danchip |
---|---|
Etch rate of PECVD BPSG | 39.4nm/min (22-01-2016) |
Selectivity to resist [:1] | Not known |
Wafer uniformity (100mm) | Not known |
Profile [o] | Not known |
Wafer uniformity map (click on the image to view a larger image) | Not known |
SEM profile images | NONE |
Comment |