Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide/IBSD of SiO2: Difference between revisions
Jump to navigation
Jump to search
No edit summary |
No edit summary |
||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/IBSD_of_SiO2 click here]''' | '''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/IBSD_of_SiO2 click here]''' | ||
[[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300|Go to IBE/IBSD Ionfab 300 equipment page]] | |||
Revision as of 09:27, 11 January 2016
Feedback to this page: click here
Go to IBE/IBSD Ionfab 300 equipment page
Acceptance test for SiO2 deposition (2011):
. | Acceptance Criteria |
Acceptance Result 1 |
Acceptance Result 2 |
---|---|---|---|
Substrate information |
|
|
|
Material to be deposited |
The purpose of the SiO2 is to be part of a mirror: <br\> 5 quarterwavelength pairs of <br\> SiO2 <br\> TiO2 <br\> Extra quarterwavelength layer of <br\> TiO2 <br\> 5 quarterwavelength pairs of <br\> SiO2 <br\> TiO2 <br\> Design wavelength (for refractive indices and layer thicknesses): 1300nm <br\> The acceptance criteria is set up for the single SiO2 and TiO2 layers. <br\> Five runs in a row for each material. |
|
|
Deposition thickness |
|
|
|
Deposition rate |
|
One standard deviation |
Only made once |
Thickness uniformity |
|
|
|
Reproducibility |
|
|
|
Stress |
|
|
|
Refractive index | . |
|
|
Recipe 1 | Recipe 2 | |
---|---|---|
Platen angle | 15 degrees | 10 degrees |
Platen rotation speed | 20rpm | 20rpm |
Ar(N) flow | 4 sccm | 4 sccm |
Ar(dep. source) flow | 9 sccm | 8 sccm |
I(N) | 310mA | 320mA |
Power | 675W | 700W |
I(B) | 310mA | 280mA |
V(B) | 1200V | 1100V |
Vacc(B) | 400V | 400V |
Deposition time | 29min | 37min |
Other results
Roughness of the surface
Measured with the Optical profiler - PSI mode (on one sample from the acceptace test): Sa= 0.6nm