(Created page with "The standard recipe for oxide etching with photo resist as masking material is called: SiO2_res. The parameters and results so fare are as follows: {| border="1" cellspacing="...")
 
No edit summary
Line 1: Line 1:
The standard recipe for oxide etching with photo resist as masking material is called: SiO2_res. The parameters and results so fare are as follows:
'''The standard recipe for oxide etching with photo resist as masking material is called: SiO2_res. The parameters and results so fare are as follows:'''
{| border="1" cellspacing="2" cellpadding="2"  
{| border="1" cellspacing="2" cellpadding="2"  
|-style="background:Black; color:White"
|-style="background:Black; color:White"

Revision as of 12:47, 19 November 2015

The standard recipe for oxide etching with photo resist as masking material is called: SiO2_res. The parameters and results so fare are as follows:

Parameter Recipe name: SiO2_res (SiO2 etch with resist mask) Variations over SiO2_res made in 2010 by BGHE
Coil Power [W] 1300 1000-1600
Platen Power [W] 200 150-300
Platen temperature [oC] 0 0
He flow [sccm] 174 174, 300
C4F8 flow [sccm] 5 5
H2 flow [sccm] 4 0, 4
Pressure [mTorr] 4 2.3, 4

Etch rates in different materials using the standard "Silicon oxide etch with resist mask"

Material to be etched Etch rate using SiO2_res
Thermal oxide ~230nm/min (5% etch load) - etch load dependency see here
TEOS oxide (5% load) 233nm/min ±0.7% - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by LN/BGE@danchip
PECVD1 (standard) oxide (5% load) 242nm/min ±0.6% - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by LN/BGE@danchip
Al2O from the ALD 50nm can be etched in 10min - etched in November 2014 by FRSTO@danchip
Silicon rich nitride from furnace B2 136nm was etched in 1min (whole wafer) - etched in October 2015 by bghe@danchip


Using different resist masks: results using the standard recipe for "Silicon oxide etch with resist mask" Section under construction.jpg

. Az MIR nLof KRF CSAR
Selectivity to thermal oxide [:1]
  • 2-3 - etch load dependency see here
  • 1.9 - tested November 2015 by BGHE
1.8 - tested November 2015 by BGHE 2.0 - tested November 2015 by BGHE ~2 - tested May 2013 by Christian Østergaard @nanotech. .
Profile [o] ~90 . . . .
Roughness of the resist after etch - striation on sidewalls . . . . .
Images See here . . See images here .
Comments A negative resist process was done to make the mask. I have not had so good results with a positive resist process. . . . Using the standard oxide recipe (SiO2_res) for 1 min the CSAR looked burned and could not be removed by CSAR stripper (AR600-71). For a better recipe look here


Striation: Side wall roughness