Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using RIE1 or RIE2: Difference between revisions
Line 190: | Line 190: | ||
{| border="2" cellspacing="1" cellpadding="3" align="center" | {| border="2" cellspacing="1" cellpadding="3" align="center" | ||
! | ! | ||
!Expected results in RIE1 | !Expected results in RIE1 (HAS BEEN DECOMMISSIONED) | ||
!Expected results in RIE2 | !Expected results in RIE2 | ||
|- | |- | ||
|Etch rate in SiO<sub>2</sub> | |Etch rate in SiO<sub>2</sub> | ||
|~120 nm/min | |style="background:WhiteSmoke; color:silver"| | ||
~120 nm/min | |||
|~120 nm/min | |~120 nm/min | ||
|- | |- | ||
|Etch rate burned resist | |Etch rate burned resist | ||
|? | |style="background:WhiteSmoke; color:silver"| | ||
? | |||
|? | |? | ||
|- | |- | ||
|Etch rate in Si<sub>3</sub>N<sub>4</sub> | |Etch rate in Si<sub>3</sub>N<sub>4</sub> | ||
|? | |style="background:WhiteSmoke; color:silver"| | ||
? | |||
|? | |? | ||
|- | |- | ||
|Etch rate in P-Si (when used as mask) | |Etch rate in P-Si (when used as mask) | ||
|? nm/min | |style="background:WhiteSmoke; color:silver"| | ||
? nm/min | |||
|? nm/min | |? nm/min | ||
|- | |- | ||
|Etch rate in Si | |Etch rate in Si | ||
(etching down to Si) | (etching down to Si) | ||
|? | |style="background:WhiteSmoke; color:silver"| | ||
? | |||
|? | |? | ||
|- | |- | ||
|Images | |Images | ||
|[[/Images of 1SIO2mbr with p-Si mask|Etches with p-Si as masking material]] | |style="background:WhiteSmoke; color:silver"| | ||
[[/Images of 1SIO2mbr with p-Si mask|Etches with p-Si as masking material]] | |||
[[/Images of 1SIO2mbr with burned resist mask|Etches with burned resist as masking material]] | [[/Images of 1SIO2mbr with burned resist mask|Etches with burned resist as masking material]] | ||
|[[/Images of 1SIO2mbr with burned resist mask|Etches with burned resist as masking material]] | |[[/Images of 1SIO2mbr with burned resist mask|Etches with burned resist as masking material]] |
Revision as of 15:29, 22 April 2014
Feedback to this page: click here
RIE (Reactive Ion Etch) can be used for etching silicon oxide. The etch is anisotropic with vertical or angled sidewalls depending on the process recipe and the masking material and geometry. The SiO2 is etched by flour radicals assisted by ion bombardment.
The substrate:
Most be a wafer of 4" or below or small pieces, not higher than about 2mm.
The silicon can be masked by these materials:
- Photoresist
- E-beam resist
- Silicon
- Silicon Nitride
- Aluminium
- Chromium (ONLY RIE2!)
- Other metals if they cover less than 5% of the wafer area (ONLY RIE2!)
Most used recipes:
QC results
Quality Controle (QC) for RIE2 - oxide etch | ||||||||||||||||||||
|
Resist as masking material:
Recipe: | 1SiO2mre |
---|---|
Masking material | Photoresist |
CF4 flow | 14 sccm |
CHF3 flow | 26 sccm |
Pressure | 100 mTorr |
RF-power | 60 W |
Expected results in RIE1 (has been decommissioned) | Expected results in RIE2 | |
---|---|---|
Etch rate in SiO2 |
~20-30 nm/min |
~20-30 nm/min |
Etch rate in Si3N4 | ? | ? |
Etch rate in P-Si (when used as mask) |
~30 nm/min |
~30 nm/min |
Etch rate in Si
(etching down to Si) |
Expected <2 nm/min |
Expected <2 nm/min |
mre:mask resist
PolySilicon as masking material
Recipe: | 1SiO2msi |
---|---|
Masking material | Silicon |
CF4 flow | 8 sccm |
CHF3 flow | 40 sccm |
Pressure | 150 mTorr |
RF-power | 150 W |
Expected results in RIE1 (HAS BEEN DECOMMISSIONED) | Expected results in RIE2 | |
---|---|---|
Etch rate in SiO2 |
~70-80 nm/min |
~70-80 nm/min |
Etch rate in Si3N4 | ? | ? |
Etch rate in P-Si (when used as mask) |
~20-30 nm/min |
~20-30 nm/min |
Etch rate in Si
(etching down to Si) |
? | ? |
Images | Etches with p-Si as masking material |
msi:mask silicon
The recipe: 1SiO2bre (se below) can also be used with p-Si as masking material.
Burned resist as masking material (developed for waveguides by Haiyan Ou @DTU Photonics):
Recipe: | 1SiO2mbr |
---|---|
Masking material | Burned resist (250oC 1h) |
CHF3 flow | 84 sccm |
Pressure | 60 mTorr |
RF-power | 200 W |
Expected results in RIE1 (HAS BEEN DECOMMISSIONED) | Expected results in RIE2 | |
---|---|---|
Etch rate in SiO2 |
~120 nm/min |
~120 nm/min |
Etch rate burned resist |
? |
? |
Etch rate in Si3N4 |
? |
? |
Etch rate in P-Si (when used as mask) |
? nm/min |
? nm/min |
Etch rate in Si
(etching down to Si) |
? |
? |
Images |
Etches with p-Si as masking material Etches with burned resist as masking material |
Etches with burned resist as masking material |
mbr:mask burned resist
A survey of the parameter space using photoresist as masking material
A DOE has been performed. A short summery is given here: (in progress)
RIE1:
A Design Of Experiment (DOE) has been performed. A screening experiment: full factorial with to levels: 9 different runs and 3 repetitions. Results from a screening experiment should be taken "with a gain of salt" meaning use it only as a rough guide line and test your recipe before use.
The Design of the experiment
|
Etch rate |
---|
Selectivity to photoresist
|
---|
Etch profile angle <br\> The etch profile was also examined but there was not found any significant correlation between the profile angle and the process parameters.