Specific Process Knowledge/Etch/Etching of Chromium: Difference between revisions
Line 22: | Line 22: | ||
|HNO<math>_3</math>:H<math>_2</math>O:cerisulphate - 90ml:1200ml:15g | |HNO<math>_3</math>:H<math>_2</math>O:cerisulphate - 90ml:1200ml:15g | ||
|Commercial chromium etch | |Commercial chromium etch | ||
CE 8002-A | |||
|- | |- | ||
|Process temperature | |Process temperature |
Revision as of 16:25, 17 January 2008
Etching of Chromium
Etching of chromium is done wet at Danchip. We have two solution for this:
- HNO:HO:cerisulphate - 90ml:1200ml:15g
- Commercial chromium etch
Etch rate 400-1000 Å/min (depending on the level of oxidation of the metal)
Chromium etch 1 | Chromium etch 2 | |
---|---|---|
General description |
Etch of chromium |
Etch of chronium |
Chemical solution | HNO:HO:cerisulphate - 90ml:1200ml:15g | Commercial chromium etch
CE 8002-A |
Process temperature | Room temperature | Room temperature |
Possible masking materials: |
Photoresist (1.5 µm AZ5214E) |
Photoresist (1.5 µm AZ5214E) |
Etch rate |
~1-2 nm/min (Pure Al) |
~60(??) nm/min |
Batch size |
1-25 wafers at a time |
1-25 wafer at a time |
Size of substrate |
4" wafers |
4" wafers |
Allowed materials |
|
|