Specific Process Knowledge/Thin film deposition/Deposition of Chromium: Difference between revisions
No edit summary |
No edit summary |
||
Line 41: | Line 41: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! Layer thickness | ! Layer thickness | ||
|10Å to 1µm | |10Å to 1µm* | ||
|10Å to 1µm | |10Å to 1µm* | ||
|10Å to 1000 Å | |10Å to 1000 Å | ||
|. | |. | ||
Line 63: | Line 63: | ||
|- | |- | ||
|} | |} | ||
'''*''' ''For thicknesses above 200 nm permission from ThinFilm group is required.'' | |||
== Studies of Cr deposition processes == | == Studies of Cr deposition processes == |
Revision as of 17:07, 6 March 2014
Feedback to this page: click here
Chromium deposition
Chromium can be deposited by e-beam evaporation. It should be noted that Chromium does not melt but evaporates directly from the solid phase. Chromium can be sputter deposited aswell. In the chart below you can compare the different deposition equipment.
E-beam evaporation (Alcatel) | E-beam evaporation (Wordentec) | E-beam evaporation (PVD co-sputter/evaporation) | Sputter deposition (Wordentec) | |
---|---|---|---|---|
Batch size |
|
|
|
|
Pre-clean | RF Ar clean | RF Ar clean | RF Ar clean | RF Ar clean |
Layer thickness | 10Å to 1µm* | 10Å to 1µm* | 10Å to 1000 Å | . |
Deposition rate | 2Å/s to 15Å/s | 10Å/s to 15Å/s | About 1Å/s | Depending on process parameters, see here. |
Comment | Only very thin layers (up to 100nm). |
* For thicknesses above 200 nm permission from ThinFilm group is required.
Studies of Cr deposition processes
Uniformity of Cr layers - Uniformity of Cr layers deposited with different methods and settings
Sputtering of Cr in Wordentec - Settings and deposition rates