Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300/IBE Au etch: Difference between revisions
No edit summary |
No edit summary |
||
Line 113: | Line 113: | ||
[[image:IBE acceptance S18-AU-ZEP5.jpg|450x450px|thumb|center|s18-Au-ZEP5]] | [[image:IBE acceptance S18-AU-ZEP5.jpg|450x450px|thumb|center|s18-Au-ZEP5]] | ||
|} | |} | ||
==IBE Au etch with Ti mask== |
Revision as of 14:32, 28 August 2013
Results from the acceptance test in February 2011
Acceptance test for Au etch:
. | Acceptance Criteria |
Acceptance Results |
---|---|---|
Substrate information |
|
. |
Material to be etched |
|
. |
Mask information |
|
. |
Features to be etched |
|
. |
Etch depth |
|
|
Etch rate |
|
|
Etch rate uniformity |
|
|
Reproducibility |
|
|
Selectivity (Au etch rate/ZEP etch rate) |
|
|
Etch profile |
|
|
Process parameters for the acceptance test
Parameter | Au etch acceptance |
---|---|
Neutalizer current [mA] | 550 |
RF Power [W] | 1300 |
Beam current [mA] | 500 |
Beam voltage [V] | 600 |
Beam accelerator voltage | 400 |
Ar flow to neutralizer [sccm] | 5.0 |
Ar flow to beam [sccm] | 10.0 |
Rotation speed [rpm] | 20 |
Stage angle [degrees] | 30 |
Some SEM profile images of the etched Au