Specific Process Knowledge/Etch/ASE (Advanced Silicon Etch): Difference between revisions
Line 74: | Line 74: | ||
The process runs for 31 cycles (5:56 mins). The fact that it's Bosch process is clear from the scallops on the sidewalls - one should be able to count 31 of them. | The process runs for 31 cycles (5:56 mins). The fact that it's Bosch process is clear from the scallops on the sidewalls - one should be able to count 31 of them. | ||
<gallery caption="Standardization images of the shallolr recipe" widths="300px" heights="300px" perrow="2"> | <gallery caption="Standardization images of the shallolr recipe" widths="300px" heights="300px" perrow="2"> | ||
Line 80: | Line 79: | ||
image:jmlshal070921 pos1 50mu_08.jpg|The profile of a 50 <math>\mu</math>m trench | image:jmlshal070921 pos1 50mu_08.jpg|The profile of a 50 <math>\mu</math>m trench | ||
</gallery> | </gallery> | ||
The process is designed to reach 20 <math>\mu</math>m down in a 2 <math>\mu</math>m trench but as is clear from the image of the corresponding 50 <math>\mu</math>m trench, this one is etched deeper. The reason is the so called Aspect Ratio Dependent Etching or ARDE. | |||
=== Deepetch === | === Deepetch === |
Revision as of 16:30, 11 December 2007
The ASE
The ICP-DRIE (Inductively Coupled Plasma - Deep Reactive Ion Etcher) tool at Danchip is manufactured by STS and is called the ASE (Advanced Silicon Etcher). The main purpose of the ASE is etching of silicon using Bosch process.
The Bosch process: Etching of silicon
The Bosch process uses alternation between an etch cycle and a passivation cycle. Introducing a passivation step in an etch process is very beneficial for the control of the angle of the sidewalls in the etch process because it allows us to cover them with a protective layer that suppresses the isotropic etching. Combined with the high plasma density in the ICP chamber, the excellent sidewall control enables us to etch high aspect ratio structures in silicon with very high etch rates.
In the case of the silicon etching on the ASE, an etch phase with SF6 and O2 alternates with a passivation phase with C4F8.
The two standard silicon etch recipes
Two recipes have been optimized for the ASE. Their specification is on a 10 % etch load wafer with trenches.
- Shallolr: The shallow etch process will etch a 2 m opening down to make a 20 m trench.
- Deepetch: The deep etch process will etch a 50 m opening down to make a 300 m trench.
The standardization procedure on the ASE covers these two etches.
Recipes on the ASE
Shallolr
The shallolr recipe is designed to etch features (with sizes above 1 m) in silicon down to a depth that ranges from a few microns to some 50 microns. If you need to etch deeper use Deepetch or more shallow, see Nanoetches.
The recipe is given below.
Common parameters | Multiplexed parameters | |||
---|---|---|---|---|
Parameter | Setting | Parameter | Etch | Passivation |
Temperature | 10oC | SF6 Flow | 260 sccm | 0 sccm |
No. of cycles | 31 | O2 Flow | 26 sccm | 0 sccm |
Process time | 5:56 mins | C4F4 Flow | 0 sccm | 120 sccm |
APC mode | manual | RF coil | 2800 W | 1000 W |
APC setting | 86.8 % | RF Platen | 16 W | 0 W |
Cycle time | 6.5 s | 5 s |
The process runs for 31 cycles (5:56 mins). The fact that it's Bosch process is clear from the scallops on the sidewalls - one should be able to count 31 of them.
- Standardization images of the shallolr recipe
The process is designed to reach 20 m down in a 2 m trench but as is clear from the image of the corresponding 50 m trench, this one is etched deeper. The reason is the so called Aspect Ratio Dependent Etching or ARDE.
Deepetch
Common parameters | Multiplexed parameters | |||
---|---|---|---|---|
Parameter | Setting | Parameter | Etch | Passivation |
Temperature | 20oC | SF6 Flow | 230 sccm | 0 sccm |
No. of cycles | 250 | O2 Flow | 23 sccm | 0 sccm |
Process time | 54:10 mins | C4F4 Flow | 0 sccm | 120 sccm |
APC mode | manual | RF coil | 2800 W | 1000 W |
APC setting | 87.7 % | RF Platen | 19 W | 0 W |
Cycle time | 8 s | 5 s |
- Standardization images of the deepetch recipe