Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using AOE/PolySi mask/Images of m PolySi1 etches

From LabAdviser
< Specific Process Knowledge‎ | Etch‎ | Etching of Silicon Oxide‎ | SiO2 etch using AOE‎ | PolySi mask
Revision as of 12:51, 3 February 2023 by Bghe (talk | contribs)
(diff) ← Older revision | Latest revision (diff) | Newer revision → (diff)
Jump to navigation Jump to search

Feedback to this page: click here
This page is written by Berit Herstrøm @ DTU Nanolab (BGHE) if nothing else is stated

Process date: February 2012
Recipe: m_poly@60degrees
Process time: 25 min
Mask: Poly Si 1.8 µm
Etch depth: 12.5 µm
Line width mask: 25µm
Line with after etch: 21.8µm
Process date: February 2012 by bghe@nanolab
Recipe: m_poly@60degrees
Process time: 25 min
Mask: Poly Si 1.8 µm thick
Etch depth: 12.5 µm
Line width mask: 8µm
Line with after etch: 5.2µm
Process date: February 2012 bghe@nanolab
Recipe: m_poly@60degrees
Process time: 25 min
Mask: Poly Si 1.8 µm
Etch depth: 12.5 µm
Line width mask: 6µm
Line with after etch: 3.4µm
Process date: February 2012 bghe@nanolab
Recipe: m_poly@60degrees
Process time: 25 min
Mask: Poly Si 1.8 µm
Etch depth: 12.5 µm
Line width mask: 4µm
Line with after etch: 1.5µm
Sharp tip/edge is formed because the Si mask is completely etched away man the line becomes lower that the wider lines due to this.