Specific Process Knowledge/Lithography: Difference between revisions

From LabAdviser
Lgpe (talk | contribs)
Taran (talk | contribs)
 
(178 intermediate revisions by 6 users not shown)
Line 1: Line 1:
<!-- =<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=-->
{{cc-nanolab}}


[[Image:DUV_wafers.jpg|250x250px|right|frame|]]
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography click here]'''


'''Feedback to this page''': '''[mailto:photolith@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography click here]'''
[[Category: Equipment|Lithography]]
<!-- Replace "http://labadviser.danchip.dtu.dk/..." with the link to the Labadviser page-->
[[Category: Lithography]]


[[Image:DUV_wafers.jpg|500px|frameless|right|]]


__TOC__
__TOC__


 
There are four different types of lithography available at DTU Nanolab:
*[[Specific Process Knowledge/Lithography/UVLithography|UV Lithography]]
*[[Specific Process Knowledge/Lithography/DUVStepperLithography|DUV Stepper Lithography]]
*[[Specific Process Knowledge/Lithography/EBeamLithography|E-beam Lithography]]
*[[Specific_Process_Knowledge/Imprinting|Nano Imprint Lithography]]
<br clear="all" />
<br clear="all" />
=Comparing lithography methods at DTU Nanolab=


=Comparing lithography methods at DTU Danchip=
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
 
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"  
|-
|-


Line 23: Line 27:
!width="16%"| [[Specific Process Knowledge/Lithography/DUVStepperLithography|DUV Stepper Lithography]]  
!width="16%"| [[Specific Process Knowledge/Lithography/DUVStepperLithography|DUV Stepper Lithography]]  
!width="16%"| [[Specific Process Knowledge/Lithography/EBeamLithography|E-beam Lithography]]
!width="16%"| [[Specific Process Knowledge/Lithography/EBeamLithography|E-beam Lithography]]
!width="16%"| [[Specific Process Knowledge/Lithography/NanoImprintLithography|Nano Imprint Lithography]]  
!width="16%"| [[Specific_Process_Knowledge/Imprinting|Nano Imprint Lithography]]  
|-
|-


Line 30: Line 34:
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!Generel description
!Generel description
|Pattern transfer via UltraViolet (UV) light
|Pattern transfer via ultraviolet (UV) light
|Pattern transfer via DeepUltraViolet (DUV) light
|Pattern transfer via deep ultraviolet (DUV) light
|Patterning by electron beam
|Patterning by electron beam
|Pattern transfer via hot embossing (HE)
|Pattern transfer via hot embossing (HE)
Line 41: Line 45:
!Pattern size range
!Pattern size range
|
|
*Resist type, thickness, and pattern dependent
~0.6 µm and up<br>
*~1.25 µm and up
(resist type, thickness, and pattern dependent)
|
|
*pattern type, shape and pitch dependent
~200 nm and up<br>
*~200 nm and up
(pattern type, shape and pitch dependent)
|
|
*~12 nm - 1 µm
~12 nm - 1 µm<br>
(and larger at high currents)
|
|
*~20 nm and up
~20 nm and up
|-
|-


Line 56: Line 61:
!Resist type
!Resist type
|
|
*UV sensitive:
UV sensitive:
**AZ 5214E, AZ 4562, AZ MiR 701 (positive)
*AZ 5214E, AZ 4562, AZ MiR 701 (positive)
**AZ 5214E, AZ nLOF 2020, SU-8 (negative)
*AZ 5214E, AZ nLOF 2020, SU-8 (negative)
|
|
*DUV sensitive
DUV sensitive
**JSR KRF M230Y, JSR KRF M35G (positive)
*JSR KRF M230Y, JSR KRF M35G (positive)
**UVN2300-0.8 (negative)
*UVN2300-0.8 (negative)
|
|
*E-beam sensitive
E-beam sensitive
**AR-P6200 CSAR, ZEP502A , PMMA, HSQ, mr-EBL, AR-N 7520
*AR-P6200 CSAR, ZEP502A , PMMA (positive)
*HSQ, mr-EBL, AR-N 7520 (negative)
|
|
*Imprint polymers:
Imprint polymers:
**Topas
*Topas
**PMMA
*PMMA
*mr-I 7030R
|-
|-


Line 76: Line 83:
!Resist thickness range
!Resist thickness range
|
|
~0.5µm to 20µm
~0.5 µm to 200 µm
|
|
~50nm to 2µm
~50 nm to 2 µm
|
|
~30nm to 0.5 µm
~30 nm to 1 µm
|
|
~ 100nm to 2µm
~ 100 nm to 2 µm
|-
|-


Line 89: Line 96:
!Typical exposure time
!Typical exposure time
|
|
2s-30s pr. wafer
10 s - 3 min pr. wafer using mask aligners<br>
10 min - 5 hours pr. wafer using maskless aligners
|
|
Process depended, depends on pattern, pattern area and dose
Process dependent:
*Pattern
*Pattern area
*Dose
 
Throughput is up to 60 wafers/hour
|
|
Depends on dose, Q [µC/cm2], beam current, I [A], and pattern area, A [cm2]:    t = Q*A/I
Process dependent:
*Dose, Q [µC/cm<sup>2</sup>]
*Beam current, I [A]
*Pattern area, a [cm<sup>2</sup>]
 
time [s] = Q*a/I
|
|
Process depended, depends also on heating and cooling temperature rates
Process dependent, including heating/cooling rates
|-
|-


Line 103: Line 121:
!Substrate size
!Substrate size
|
|
*small samples
*chips down to 3 mm x 3 mm
*50 mm wafers
*50 mm wafers
*100 mm wafers
*100 mm wafers
*150 mm wafers  
*150 mm wafers  
*200 mm wafers
|
|
*100 mm wafers
*100 mm wafers
Line 112: Line 131:
*200 mm wafers
*200 mm wafers
|
|
We have cassettes that fit to
We have cassettes fitting:
*4 small samples (20mm, 12mm, 8mm, 4mm)
*4 small samples (slit openings: 20mm, 12mm, 8mm, 4mm)
*6 wafers of 50 mm in size
*6 wafers of 50 mm in size
*3 wafers of 100 mm in size
*3 wafers of 100 mm in size
*1 wafer of 150 mm in size  
*1 wafer of 150 mm in size  
*1 wafer of 200 mm in size
*1 wafer of 200 mm in size
Only one cassette can be loaded at time
Only one cassette can be loaded at a time
|
|
*small samples
*small samples
Line 129: Line 148:
!'''Allowed materials'''
!'''Allowed materials'''
|
|
*Any standard cleanroom material  
Any standard cleanroom material  
|
|
*Any standard cleanroom material  
Any standard cleanroom material  
|
|
*Any standard cleanroom material  
Any standard cleanroom material, except:
*Materials that will degas
*Graphene requires special treatment 
|
|
*Any standard cleanroom material  
Any standard cleanroom material  
|-
|-
|}
|}
<br clear="all" />
<br clear="all" />


=Equipment Pages=
=Equipment Pages=


{| style="color: black;" width="90%"
{| style="color: black;" width="90%"
Line 149: Line 167:
|-
|-
| style="width: 20%"|
| style="width: 20%"|
'''<big>[[Specific Process Knowledge/Lithography/Resist|Resist]]</big>'''
*[[Specific_Process_Knowledge/Lithography/Resist#User_resist_bottles_in_the_cleanroom|User bottles in the cleanroom]]
*[[Specific_Process_Knowledge/Lithography/Resist#UV_Resist|UV Resist]]
*[[Specific_Process_Knowledge/Lithography/Resist#DUV_Resist|DUV Resist]]
*[[Specific_Process_Knowledge/Lithography/Resist#E-beam_Resist|E-beam Resist]]
*[[Specific_Process_Knowledge/Lithography/Resist#Imprint_Resist|Imprint Resist]]
'''<big>[[Specific Process Knowledge/Lithography/Pretreatment|Pretreatment]]</big>'''
'''<big>[[Specific Process Knowledge/Lithography/Pretreatment|Pretreatment]]</big>'''
*[[Specific Process Knowledge/Lithography/Pretreatment#HMDS|HMDS]]
*[[Specific Process Knowledge/Lithography/Pretreatment#HMDS|HMDS]]
*[[Specific Process Knowledge/Lithography/Pretreatment#BHF|BHF]]
*[[Specific Process Knowledge/Lithography/Pretreatment#Buffered_HF-Clean|BHF]]
*[[Specific_Process_Knowledge/Lithography/Pretreatment#Oven_250C|Oven 250C]]
*[[Specific_Process_Knowledge/Lithography/Pretreatment#Oven_250C|Oven 250C]]


'''<big>[[Specific Process Knowledge/Lithography/Coaters|Coating]]</big>'''
'''<big>[[Specific Process Knowledge/Lithography/Coaters|Coating]]</big>'''
*[[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV|Spin Coater: Gamma UV]]
*[[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV|Spin Coater: Gamma UV]]
*[[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_E-beam_and_UV|Spin Coater: Gamma e-beam & UV]]
*[[Specific Process Knowledge/Lithography/Coaters#Spin_Coater:_RCD8|Spin Coater: RCD8]]
*[[Specific Process Knowledge/Lithography/Coaters#Spin_Coater:_RCD8|Spin Coater: RCD8]]
*[[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: Manual/Labspin ...]]
*[[Specific_Process_Knowledge/Lithography/Coaters#Spin_coater:_Labspin|Spin Coater: Labspin 02/03]]
*[[Specific_Process_Knowledge/Lithography/Coaters/SprayCoater|Spray Coater]]
*[[Specific_Process_Knowledge/Lithography/Coaters/SprayCoater|Spray Coater]]
*[[Specific Process Knowledge/Lithography/DUVStepperLithography#SÜSS Spinner-Stepper|Spin coater: Süss Stepper]]
*[[Specific Process Knowledge/Lithography/DUVStepperLithography#SÜSS Spinner-Stepper|Spin coater: Süss Stepper]]
*[[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_E-beam_and_UV|Spin Coater: Gamma e-beam & UV]]


'''<big>[[Specific Process Knowledge/Lithography/Baking|Baking]]</big>'''
'''<big>[[Specific Process Knowledge/Lithography/Baking|Baking]]</big>'''
Line 166: Line 191:
*[[Specific Process Knowledge/Lithography/Baking#Ovens|Ovens]]
*[[Specific Process Knowledge/Lithography/Baking#Ovens|Ovens]]


| style="width: 20%"|
| style="width: 20%"; valign="top"|
'''<big>[[Specific Process Knowledge/Lithography/UVExposure|UV Exposure]]</big>'''
'''<big>[[Specific Process Knowledge/Lithography/UVExposure|UV Exposure Tools]]</big>'''
*[[Specific Process Knowledge/Lithography/UVExposure#KS Aligner|KS Aligner]]
*[[Specific Process Knowledge/Lithography/UVExposure#KS Aligner|KS Aligner]]
*[[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|Aligner: MA6-2]]
*[[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|Aligner: MA6-2]]
*[[Specific Process Knowledge/Lithography/UVExposure#Aligner-6inch|Aligner: 6inch]]
<!--*[[Specific Process Knowledge/Lithography/UVExposure#Inclined UV lamp|Inclined UV-lamp]]-->
*[[Specific Process Knowledge/Lithography/UVExposure#Inclined UV lamp|Inclined UV-lamp]]
*[[Specific Process Knowledge/Lithography/UVExposure#Aligner: Maskless 01|Aligner: Maskless 01]]
*[[Specific Process Knowledge/Lithography/UVExposure#Aligner: Maskless 01|Aligner: Maskless 01]]
*[[Specific Process Knowledge/Lithography/UVExposure#Aligner: Maskless 02|Aligner: Maskless 02]]
*[[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_03|Aligner: Maskless 03]]


'''<big>[[Specific Process Knowledge/Lithography/UVExposure|Deep-UV Exposure]]</big>'''
'''<big>[[Specific_Process_Knowledge/Lithography/DUVStepperLithography|Deep-UV Exposure]]</big>'''
*[[Specific_Process_Knowledge/Lithography/DUVStepperLithography#DUV_Stepper|DUV Stepper (Canon FPA-3000EX4)]]
*[[Specific_Process_Knowledge/Lithography/DUVStepperLithography#DUV_Stepper|DUV Stepper (Canon FPA-3000EX4)]]


'''<big>[[Specific Process Knowledge/Lithography/EBeamLithography|Electron Beam Exposure]]</big>'''
'''<big>[[Specific Process Knowledge/Lithography/EBeamLithography|Electron Beam Exposure]]</big>'''
*[[Specific_Process_Knowledge/Lithography/EBeamLithography/JEOL_JBX-9500FSZ|E-Beam Writer 9500 (JEOL JBX-9500FSZ)]]
*[[Specific_Process_Knowledge/Lithography/EBeamLithography/JEOL_9500_User_Guide|JEOL 9500]]
*[[Specific_Process_Knowledge/Lithography/EBeamLithography/RaithElphy|Raith Elphy on SEM - LEO]]
*[[Specific_Process_Knowledge/Lithography/EBeamLithography/eLINE|Raith Eline]]
 
'''<big>[[Specific_Process_Knowledge/Imprinting|Nano Imprint Lithography]]</big>'''
*[[Specific Process Knowledge/Thin film deposition/MVD|Molecular Vapour Deposition]]
*[[Specific Process Knowledge/Lithography/NanoImprintLithography#EVG NIL|Imprinter 01]]
 


| style="width: 20%"; valign="top"|
'''<big>[[Specific Process Knowledge/Lithography/Development|Development]]</big>'''
'''<big>[[Specific Process Knowledge/Lithography/Development|Development]]</big>'''
*[[Specific Process Knowledge/Lithography/Development#Developer-6inch|Developer: 6inch]]
*[[Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography|Developer: TMAH UV-lithography]]
*[[Specific Process Knowledge/Lithography/Development#SU8-Developer|Developer: SU8]]
*[[Specific_Process_Knowledge/Lithography/Development#Developer:_TMAH_Manual|Developer: TMAH Manual]]
*[[Specific_Process_Knowledge/Lithography/Development#Developer:_TMAH_Manual|Developer: TMAH Manual]]
*[[Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography|Developer: TMAH UV-lithography]]
*[[Specific Process Knowledge/Lithography/Development#Developer:_SU8_(wetbench)|Developer: SU8 (wetbench)]]
*[[Specific_Process_Knowledge/Lithography/DUVStepperLithography#Developer_TMAH_Stepper|Developer: TMAH Stepper]]
*[[Specific_Process_Knowledge/Lithography/DUVStepperLithography#Developer:_TMAH_Stepper|Developer: TMAH Stepper]]
*[[Specific_Process_Knowledge/Lithography/Development#Developer:_E-beam|Developer: E-beam]]


| style="width: 20%"|
'''<big>[[Specific Process Knowledge/Lithography/Descum|Descum]]</big>'''
'''<big>[[Specific Process Knowledge/Lithography/Strip|Strip]]</big>'''
*[[Specific Process Knowledge/Lithography/Descum#Plasma_Asher_1|Plasma Asher 1]]
*[[Specific Process Knowledge/Lithography/Strip#Plasma Asher 1|Plasma Asher 1]]
*[[Specific Process Knowledge/Lithography/Descum#Plasma_Asher_2|Plasma Asher 2]]
*[[Specific Process Knowledge/Lithography/Strip#Plasma Asher 2|Plasma Asher 2]]
*[[Specific Process Knowledge/Lithography/Descum#Plasma_Asher_3:_Descum|Plasma Asher 3:Descum]]
*[[Specific Process Knowledge/Lithography/Strip#III-V Plasma Asher|III-V Plasma Asher]]
*[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)|BHF]]
*[[Specific Process Knowledge/Lithography/Strip#Rough Acetone Strip|Resist Strip]]


'''<big>[[Specific Process Knowledge/Lithography/LiftOff|Lift-off]]</big>'''
'''<big>[[Specific Process Knowledge/Lithography/LiftOff|Lift-off]]</big>'''
*[[Specific Process Knowledge/Lithography/LiftOff#LiftOff|Lift-off]]
*[[Specific Process Knowledge/Lithography/LiftOff#Lift-off_wet_bench_07|Lift-off]]
 
'''<big>[[Specific_Process_Knowledge/Lithography/NanoImprintLithography|NanoImprint Lithography]]</big>'''
*[[Specific Process Knowledge/Thin film deposition/MVD|Molecular Vapour Deposition]]
*[[Specific Process Knowledge/Lithography/NanoImprintLithography#EVG NIL|Imprinter 01]]


'''<big>[[Specific Process Knowledge/Lithography/Strip|Strip]]</big>'''
*[[Specific Process Knowledge/Lithography/Strip#Plasma_Asher_1|Plasma Asher 1]]
*[[Specific Process Knowledge/Lithography/Strip#Plasma_Asher_2|Plasma Asher 2]]
*[[Specific Process Knowledge/Lithography/Strip#Plasma_Asher_3: Descum|Plasma Asher 3: Descum]]
*[[Specific Process Knowledge/Lithography/Strip#Resist_Strip|Resist Strip]]
|}
|}
<br clear="all" />
<br clear="all" />


=Lithography Tool Package Training=
=Lithography Tool Package Training=


DTU Nanolab offers a Tool Package Training in Lithography; the course includes theory on lithographic processes and equipment. After the TPT has been successfully completed, you can begin training on the lithography equipment at DTU Nanolab.


DTU Danchip offers a Tool Package Training in Lithography; the course includes theory on lithographic processes and equipment, as well as training in equipment operation and processing in the cleanroom.  
You are required to pass this course, in order to get access to using the lithography equipment inside the DTU Nanolab fabrication facility (The Cleanroom).


The course is for all users that intend to perform any kind of lithographic processing in the cleanroom, and is a prerequisite for training in other lithography equipment.
For details, dates, and course material, please check the course description under [[LabAdviser/Courses#The_Lithography_TPT|Courses]].
 
 
'''For details, dates, and course material, please check the course description under [[LabAdviser/Courses#The_Lithography_TPT|Courses]].'''
 
 
{|border="1" cellspacing="0" cellpadding="3" align="left" style="text-align:left;" style="width: 70%;"
|-
 
|-
|-style="background:White; color:black; text-align:center"
!colspan="2"|Lithography Tool Package Training
|-


|-
!Schedule
|
<!--'''<span style="color: red;">OBS: The December Litho TPT has been cancelled due to sickness. Contact the Lithography Group for rescheduling if this poses a problem.</span>''' <span style="text-decoration: line-through;">'''NEXT LECTURE: Tuesday 29th of November 9:15 - 13:00 (B347, Seminar room)'''</span>-->
'''Theoretical part'''
<!--* The lecture has been replaced by videos that can be viewed at one's leisure.-->
* A 1 hour "questions and exercises" session once or twice a month will be planned as needed (typically Fridays 09:30-10:30).
<!--* NEXT "questions and exercises" sessions: '''24th of March, 31st of March, 21st of April, 28th of April, 19th of May'''-->
'''Practical part'''
* A 4-5 hour training session 2-3 times a month, max. 4 persons per session (typically Wednesdays 09:00 - 14:00).
<!--* NEXT training sessions: '''29th of March, 5th of April, 26th of April, 3rd of May, 24th of May'''-->
|-


|-
'''Signing up for the course'''
!Location
|
'''Theoretical part'''
* The location of the "questions and exercises" session will be specified after signing up for the course.
'''Practical part'''
* The training session takes place inside the cleanroom. The meeting point will be in front of the first equipment.
|-


|-
The course is in DTU Learn. You sign up for the course by enrolling yourself in the course [https://learn.inside.dtu.dk/d2l/le/discovery/view/course/56077 DTU Nanolab TPT: Lithography] - '''requires login'''
!Qualified Prerequisites
* Watch the lecture videos
|
* Successfully complete all the quizzes
* Cleanroom safety course at DTU Danchip
* Admission to the cleanroom must be obtained before the training session
|-


|-
!Preparations
|
'''Before the "questions and exercises" session'''
* Read Sami Franssila "Introduction to Microfabrication" (2010), Chapter 9: Optical Lithography. (Available online from DTU campus)
* Watch the lecture videos (7 videos, 2:41 hours in total). Write down any questions that may arise during the videos.
'''Before training session'''
* Watch the training videos of spin coating (automatic), exposure (operation, and alignment), and development (automatic).
* Study the equipment manuals. The manuals are available in LabManager.
* Study the TPT process flows (first print, and alignment).
<!--'''Links to literature, lecture videos, training videos, equipment manuals, and process flows can be found in the "Knowledge and Information" section below.'''-->
|-


|-
'''Learning objectives'''
!Course Responsible
|
The Lithography Group at DTU Danchip.


Sign up for the course by e-mailing to [mailto:lithography@danchip.dtu.dk lithography@danchip.dtu.dk].
Learn about the fundamentals of lithography processing in a cleanroom fabrication lab:
|-
* Coating
* Exposure
* Development
* Resist, substrates and pre-treatment
* Post-lithography steps


|-
!Learning Objectives
|
* Describe fundamental parts of lithographic processing in a cleanroom, design of process flows
* Authorization to use spin coater, mask aligner, and developer at DTU Danchip
* Calculate relevant process parameters
* Analyze and apply your results of lithographic processing
|-


|}
'''After completing the TPT'''


When all TPT quizzes have been completed successfully, you have finished the lithography TPT, and can begin the online training on the lithography equipment you need to use. The online training is available in the course [https://learn.inside.dtu.dk/d2l/le/discovery/view/course/118192 DTU Nanolab: lithography equipment training] - '''requires login'''


After completing the online equipment training, you become eligible for the hands-on authorization training, which will take place inside the cleanroom.
<br clear="all" />
<br clear="all" />


Line 293: Line 274:
| colspan="3" |  
| colspan="3" |  
|-
|-
| style="width: 20%"|
| style="width: 20%"; valign="top"|
'''<big>Literature</big>'''
'''<big>Literature</big>'''
*[http://onlinelibrary.wiley.com/doi/10.1002/9781119990413.ch9/pdf  Franssila, 2010, Chapter 9: Optical Lithography]
*[http://onlinelibrary.wiley.com/doi/10.1002/9781119990413.ch9/pdf  Franssila, 2010, Chapter 9: Optical Lithography]
Line 301: Line 282:
*[http://www.cnf.cornell.edu/cnf_spietoc.html Handbook of Microlithography, Micromachining, and Microfabrication, Chapter 2: E-beam Lithography]
*[http://www.cnf.cornell.edu/cnf_spietoc.html Handbook of Microlithography, Micromachining, and Microfabrication, Chapter 2: E-beam Lithography]
*[http://onlinelibrary.wiley.com/doi/10.1002/9781118557662.ch3/summary Stefan Landis,Lithography, Chapter 3: E-beam Lithography]
*[http://onlinelibrary.wiley.com/doi/10.1002/9781118557662.ch3/summary Stefan Landis,Lithography, Chapter 3: E-beam Lithography]
*[https://www.microchemicals.com/downloads/application_notes.html Application notes] from MicroChemicals GmbH, e.g. [https://www.microchemicals.com/technical_information/lithography_trouble_shooting.pdf Lithography Trouble-Shooter]




'''<big>Lecture videos</big>'''
'''<big>Lecture videos</big>'''
*Lithography TPT lecture videos (7 videos, 2:41 hours in total) on [http://podcast.llab.dtu.dk/index.php?id=302 DTU Podcasts] or [https://www.youtube.com/watch?v=hMgpRSOokxE&list=PLjWVU97LayHCHDueZ8qdT1LXJLGr4wLOa YouTube]
*Lithography TPT lecture videos:
**Current version (6 videos, 1:28 hours:minutes in total) on [https://www.youtube.com/playlist?list=PLjWVU97LayHCp7x9OujmVlZWLAnK4CDFR YouTube]
**Old version (7 videos, 2:41 hours in total) on [https://www.youtube.com/watch?v=hMgpRSOokxE&list=PLjWVU97LayHCHDueZ8qdT1LXJLGr4wLOa YouTube]
*A full [https://www.youtube.com/watch?v=TdwUGOxCdUc&index=39&list=PLM2eE_hI4gSDjK4SiDbhpmpjw31Xyqfo_ lecture series] from a UT Austin course on microfabrication by "litho guru" Chris Mack. Half of the lectures are on (projection) lithography :-)
*A full [https://www.youtube.com/watch?v=TdwUGOxCdUc&index=39&list=PLM2eE_hI4gSDjK4SiDbhpmpjw31Xyqfo_ lecture series] from a UT Austin course on microfabrication by "litho guru" Chris Mack. Half of the lectures are on (projection) lithography :-)


 
| style="width: 20%"; valign="top"|
'''<big>Lithography TPT lecture slides</big>'''
<!-- Removed by TARAN 2024-09-27
*[[:Media:Litho_Tool_Package_-_Introduction.pdf|TPT slides: Introduction]]
'''<big>Lithography TPT lecture slides</big>'''<br>
*[[:Media:Litho_Tool_Package_-_Spin_coating.pdf‎|TPT slides: Spin Coating]]
''' NB: Access to slides require login'''
*[[:Media:Litho_Tool_Package_-_Exposure.pdf|TPT slides: UV Exposure]]
*[https://labmanager.dtu.dk/view_binary.php?class=MiscDocument&id=4&name=Litho_Tool_Package_-_Introduction.pdf TPT slides: Introduction]
*[[:Media:Litho_Tool_Package_-_Development.pdf‎|TPT slides: Development]]
*[https://labmanager.dtu.dk/view_binary.php?class=MiscDocument&id=4&name=Litho_Tool_Package_-_Spin_coating.pdf TPT slides: Spin Coating]
*[[:Media:Litho_Tool_Package_-_Post_processing.pdf‎|TPT slides: Post-processing]]
*[https://labmanager.dtu.dk/view_binary.php?class=MiscDocument&id=4&name=Litho_Tool_Package_-_Exposure.pdf TPT slides: UV Exposure]
*[[:Media:Litho_Tool_Package_-_Process_effects_and_examples.pdf|TPT slides: Process Effects and Examples]]
*[https://labmanager.dtu.dk/view_binary.php?class=MiscDocument&id=4&name=Litho_Tool_Package_-_Development.pdf TPT slides: Development]
 
*[https://labmanager.dtu.dk/view_binary.php?class=MiscDocument&id=4&name=Litho_Tool_Package_-_Post_processing.pdf TPT slides: Post-processing]
| style="width: 20%"|
*[https://labmanager.dtu.dk/view_binary.php?class=MiscDocument&id=4&name=Litho_Tool_Package_-_Process_effects_and_examples.pdf TPT slides: Process Effects and Examples]
-->


'''<big>Training videos</big>'''
'''<big>Training videos</big>'''
*[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.055_Spin_Coater_GAMMA_UV-720p.mp4 Training Video: Automatic Spin Coater]
*[https://www.youtube.com/watch?v=3JhM3rmLVpA Training Video: Automatic Spin Coater]
*[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.057_Manual_Spin_Coater_V2-720p.mp4 Training Video: Manual Spin Coater]
*[https://www.youtube.com/watch?v=_neUkDsQhsM: Training Video: Manual Spin Coater Labspin]
*[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.053_Aligner_MA6_part1_operation-720p.mp4 Training Video: UV Mask Aligner Part I (Operation)]
*[https://www.youtube.com/watch?v=o8IBtfQHNzU Training Video: UV Mask Aligner Part I (Operation)]
*[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.053_Aligner_MA6_part2_aligning-720p.mp4 Training Video: UV Mask Aligner Part II (Alignment)]
*[https://www.youtube.com/watch?v=rvUuXYgw-xU Training Video: UV Mask Aligner Part II (Alignment)]
*[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.050_Developer_TMAH_UV-Lithography-720p.mp4 Training Video: Automatic Puddle Developer]
*[https://www.youtube.com/watch?v=GyTQNmbev2c Training Video: Maskless aligner Training Video]
*[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.049_Developer_Manual-720p.mp4 Training Video: Manual Puddle Developer]
*[https://www.youtube.com/watch?v=Vpa9QoCHA4I Training Video: Maskless aligner Conversion]
Playlist on YouTube:
*[https://www.youtube.com/watch?v=wIF-oqVR1Dc Training Video: Maskless aligner Series and Navigation]
*[https://www.youtube.com/watch?v=3JhM3rmLVpA&list=PLjWVU97LayHCX4sz2AH_YiPbNRmkrBYe5 Lithography TPT training videos]
*[https://youtu.be/yclriey6xpM Training Video: Maskless aligner Alignment]
*[https://www.youtube.com/watch?v=fs9DRH0Eo3k Training Video: Automatic Puddle Developer]
*[https://www.youtube.com/watch?v=btinNzYnLnY Training Video: Manual Puddle Developer]
'''Playlists on YouTube:'''
*[https://www.youtube.com/watch?v=3JhM3rmLVpA&list=PLjWVU97LayHAiCabstMfAUeeWyQoQI_cV Maskless aligner training videos]
*[https://www.youtube.com/watch?v=3JhM3rmLVpA&list=PLjWVU97LayHCX4sz2AH_YiPbNRmkrBYe5 Old Lithography TPT training videos]




'''<big>Manuals</big>'''
| style="width: 20%"; valign="top"|
'''<big>Manuals</big>'''<br>
'''NB: Access to manuals require login'''
*Automatic Spin Coater: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=359 Spin Coater: Gamma UV]
*Automatic Spin Coater: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=359 Spin Coater: Gamma UV]
*Manual Spin Coater: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=331 Spin Coater: Manual Standard Resists]
*Manual Spin Coater: [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=362 Spin Coater: Labspin 02] or [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=387 Spin Coater: Labspin 03]
*UV Mask Aligner: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=339 Aligner: MA6 - 2] or [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=44 KS Aligner]
*UV Mask Aligner: [http://labmanager.dtu.dk/d4Show.php?id=3822&mach=339 Aligner: MA6 - 2] or [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=44 KS Aligner]
*Automatic Puddle Developer: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=329 Developer: TMAH UV-lithography]
*Automatic Puddle Developer: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=329 Developer: TMAH UV-lithography]
*Manual Puddle Developer: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=324 Developer: TMAH Manual]
*Manual Puddle Developer: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=324 Developer: TMAH Manual]
*Manual E-beam Developer: [http://labmanager.dtu.dk/d4Show.php?id=5070&mach=341 Developer: E-beam Manual]




'''<big>Process Flows</big>'''
'''<big>Process Flows</big>'''
*[[:Media:Process_Flow_TPT first print.pdf|TPT first print process flow]]
*[[Specific_Process_Knowledge/Lithography/Resist#UV_resist_comparison_table|UV resist process flows]]
*[[:Media:Process_Flow_TPT alignment.pdf|TPT alignment process flow]]
*[[Specific_Process_Knowledge/Lithography/EBeamLithography#E-beam_resists_and_Process_flow|E-beam resist process flows]]
 
*[[:Media:Process_Flow_TPT first print.pdf|Old TPT process flow (first print)]]
| style="width: 20%"|
*[[:Media:Process_Flow_TPT alignment.pdf|Old TPT process flow (alignment)]]
 
'''<big>Resists</big>'''
*[[Specific_Process_Knowledge/Lithography/UVLithography#Resist_Overview|UV Resist Overview]]
*[[Specific_Process_Knowledge/Lithography/EBeamLithography#E-beam_resists|E-beam Resist Overview]]
 
 
'''<big>UV Exposure</big>'''
*[[Specific_Process_Knowledge/Lithography/UVExposure_Dose|Information on UV Exposure Dose]]
 
 
'''<big>Electron Beam Exposure</big>'''
*[[Specific_Process_Knowledge/Lithography/EBeamLithography/JEOL_JBX-9500FSZ#Getting_started|Training on JEOL JBX-9500FSZ]]
*[[Specific_Process_Knowledge/Lithography/EBeamLithography#E-beam_resists_and_Process_Flows|E-beam resists and process flows]]
*[[:Media:E-beam Lithography Lecture Tine Greibe 2015.pdf|Lecture on E-beam Lithography]]
 
 
'''<big>Deep-UV Exposure</big>'''
*[[Specific_Process_Knowledge/Lithography/DUVStepperLithography|Deep-UV Stepper Lithography]]
 
|}
|}
<br clear="all" />
<br clear="all" />

Latest revision as of 12:02, 27 September 2024

The contents on this page, including all images and pictures, was created by DTU Nanolab staff unless otherwise stated.

Feedback to this page: click here

There are four different types of lithography available at DTU Nanolab:


Comparing lithography methods at DTU Nanolab

UV Lithography DUV Stepper Lithography E-beam Lithography Nano Imprint Lithography
Generel description Pattern transfer via ultraviolet (UV) light Pattern transfer via deep ultraviolet (DUV) light Patterning by electron beam Pattern transfer via hot embossing (HE)
Pattern size range

~0.6 µm and up
(resist type, thickness, and pattern dependent)

~200 nm and up
(pattern type, shape and pitch dependent)

~12 nm - 1 µm
(and larger at high currents)

~20 nm and up

Resist type

UV sensitive:

  • AZ 5214E, AZ 4562, AZ MiR 701 (positive)
  • AZ 5214E, AZ nLOF 2020, SU-8 (negative)

DUV sensitive

  • JSR KRF M230Y, JSR KRF M35G (positive)
  • UVN2300-0.8 (negative)

E-beam sensitive

  • AR-P6200 CSAR, ZEP502A , PMMA (positive)
  • HSQ, mr-EBL, AR-N 7520 (negative)

Imprint polymers:

  • Topas
  • PMMA
  • mr-I 7030R
Resist thickness range

~0.5 µm to 200 µm

~50 nm to 2 µm

~30 nm to 1 µm

~ 100 nm to 2 µm

Typical exposure time

10 s - 3 min pr. wafer using mask aligners
10 min - 5 hours pr. wafer using maskless aligners

Process dependent:

  • Pattern
  • Pattern area
  • Dose

Throughput is up to 60 wafers/hour

Process dependent:

  • Dose, Q [µC/cm2]
  • Beam current, I [A]
  • Pattern area, a [cm2]

time [s] = Q*a/I

Process dependent, including heating/cooling rates

Substrate size
  • chips down to 3 mm x 3 mm
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers

We have cassettes fitting:

  • 4 small samples (slit openings: 20mm, 12mm, 8mm, 4mm)
  • 6 wafers of 50 mm in size
  • 3 wafers of 100 mm in size
  • 1 wafer of 150 mm in size
  • 1 wafer of 200 mm in size

Only one cassette can be loaded at a time

  • small samples
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
Allowed materials

Any standard cleanroom material

Any standard cleanroom material

Any standard cleanroom material, except:

  • Materials that will degas
  • Graphene requires special treatment

Any standard cleanroom material


Equipment Pages

Resist

Pretreatment

Coating

Baking

UV Exposure Tools

Deep-UV Exposure

Electron Beam Exposure

Nano Imprint Lithography


Development

Descum

Lift-off

Strip


Lithography Tool Package Training

DTU Nanolab offers a Tool Package Training in Lithography; the course includes theory on lithographic processes and equipment. After the TPT has been successfully completed, you can begin training on the lithography equipment at DTU Nanolab.

You are required to pass this course, in order to get access to using the lithography equipment inside the DTU Nanolab fabrication facility (The Cleanroom).

For details, dates, and course material, please check the course description under Courses.


Signing up for the course

The course is in DTU Learn. You sign up for the course by enrolling yourself in the course DTU Nanolab TPT: Lithography - requires login

  • Watch the lecture videos
  • Successfully complete all the quizzes


Learning objectives

Learn about the fundamentals of lithography processing in a cleanroom fabrication lab:

  • Coating
  • Exposure
  • Development
  • Resist, substrates and pre-treatment
  • Post-lithography steps


After completing the TPT

When all TPT quizzes have been completed successfully, you have finished the lithography TPT, and can begin the online training on the lithography equipment you need to use. The online training is available in the course DTU Nanolab: lithography equipment training - requires login

After completing the online equipment training, you become eligible for the hands-on authorization training, which will take place inside the cleanroom.

Knowledge and Information about Lithography

Literature


Lecture videos

  • Lithography TPT lecture videos:
    • Current version (6 videos, 1:28 hours:minutes in total) on YouTube
    • Old version (7 videos, 2:41 hours in total) on YouTube
  • A full lecture series from a UT Austin course on microfabrication by "litho guru" Chris Mack. Half of the lectures are on (projection) lithography :-)

Training videos

Playlists on YouTube:


Manuals
NB: Access to manuals require login


Process Flows