Specific Process Knowledge/Lithography/Coaters: Difference between revisions

From LabAdviser
Jump to navigation Jump to search
Line 276: Line 276:
{{:Specific Process Knowledge/Lithography/Coaters/GammaUV}}
{{:Specific Process Knowledge/Lithography/Coaters/GammaUV}}


==Spin Coater: Gamma E-beam and UV==
{{:Specific Process Knowledge/Lithography/Coaters/GammaEbeam}}
 
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_E-beam_and_UV click here]'''
 
''[[Specific_Process_Knowledge/Lithography/Coaters#Coater_Comparison_Table|Coater comparison table]]''
 
[[image:Gamma_4M_-_E-beam_&_UV_full.JPG|400px|right|thumb|Spin Coater: Gamma E-beam & UV in E-5]]
 
Spin Coater: Gamma E-beam and UV will be installed at DTU Nanolab in June 2017. It is a Gamma 4M cluster from Süss MicroTec with spin coating, vapour priming, and baking modules. The system handles 2", 4", and 6" wafers without size conversion, using two separate coater stations.
 
The 2" coater station is equipped with 2 different resists lines:
*AZ 5214E
*AR-P 6200.09 (CSAR)
and
*1 syringe, which can be used for various resists (anisole or PGMEA-based).
 
The 4"/6" coater station is equipped with 4 different resists lines:
*AZ 5214E
*AZ MiR 701
*AR-P 6200.09 (CSAR)
*AZ 4562 
 
The processes that are available on the system are developed by Nanolab. Upon request, it is possible to establish new processes. Use of the syringe requires special training, and would as a starting point require batches in excess of 20 wafers.
 
'''[https://www.youtube.com/watch?v=3JhM3rmLVpA Training video]''' (for Spin Coater: Gamma UV)
 
'''The user manual, quality control procedures and results, user APVs, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=417 LabManager]'''
 
===Process information===
 
[[Specific Process Knowledge/Lithography/Coaters/Spin Coater: Gamma E-beam and UV processing|General Process information]]
 
[[Specific_Process_Knowledge/Lithography/Coaters/Spin_Coater:_Gamma_E-beam_and_UV_processing#Standard_Processes|Standard Processes:]]
*[[Specific_Process_Knowledge/Lithography/Coaters/Spin_Coater:_Gamma_E-beam_and_UV_processing#Quality_Control_.28QC.29|Quality Control (QC)]]
*[[Specific_Process_Knowledge/Lithography/Coaters/Spin_Coater:_Gamma_E-beam_and_UV_processing#HMDS_priming_2|HMDS]]
*[[Specific_Process_Knowledge/Lithography/Coaters/Spin_Coater:_Gamma_E-beam_and_UV_processing#AZ_5214E_coating|AZ 5214E on Coater1 and Coater2]]
*[[Specific_Process_Knowledge/Lithography/Coaters/Spin_Coater:_Gamma_E-beam_and_UV_processing#AZ_MiR_701_.2829cps.29_coating|AZ MiR 701 on Coater2]]
*[[Specific_Process_Knowledge/Lithography/Coaters/Spin_Coater:_Gamma_E-beam_and_UV_processing#AR-P_6200_.28CSAR.29_coating|CSAR on Coater1 and Coater2]]
*[[Specific_Process_Knowledge/Lithography/Coaters/Spin_Coater:_Gamma_E-beam_and_UV_processing#AZ_4562_coating|AZ 4562 on Coater2]]
*[[Specific_Process_Knowledge/Lithography/Coaters/Spin_Coater:_Gamma_E-beam_and_UV_processing#Edge_bead_removal_2|Edge bead removal on Coater1 and Coater2]]
 
[[Specific_Process_Knowledge/Lithography/Coaters/Spin_Coater:_Gamma_E-beam_and_UV_processing#Syringe_Processes|Syringe Processes]]
 
=== Equipment performance and process related parameters ===
 
{| border="2" cellspacing="0" cellpadding="2"
 
!style="background:silver; color:black;" align="center" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
*HMDS priming
*Spin coating of anisole based E-beam resists
*Spin coating of PGMEA based UV resists
*Soft baking
*Edge bead removal (CSAR and novolac-based UV resists)
|-
!style="background:silver; color:black;" align="center" width="60"|Resist
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
* AR-P 6200.09 (CSAR)
* AZ 5214E
* AZ MiR 701 (29cps) ''4"/6" only''
* AZ 4562 ''4"/6" only''
* 30cc syringe dispense ''2" only''
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Performance
|style="background:LightGrey; color:black"|HMDS contact angle
|style="background:WhiteSmoke; color:black" align="center"|
60 - 80° (on Silicon)
|-
|style="background:LightGrey; color:black"|Coating thickness
|style="background:WhiteSmoke; color:black" align="center"|
* AR-P 6200.09 (CSAR): 170-500 nm
* AZ 5214E: 1.5-5 µm
* AZ MiR 701: 1.5-4 µm
* AZ 4562: 5-25 µm
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="5"|Process parameters
|style="background:LightGrey; color:black"|Priming temperature
|style="background:WhiteSmoke; color:black" align="center"|
120 °C
|-
|style="background:LightGrey; color:black"|Spin speed
|style="background:WhiteSmoke; color:black" align="center"|
10 - 6000 rpm
|-
|style="background:LightGrey; color:black"|Spin acceleration
|style="background:WhiteSmoke; color:black" align="center"|
10 - 10000 rpm/s
|-
|style="background:LightGrey; color:black"|Hotplate temperature
|style="background:WhiteSmoke; color:black" align="center"|
25 - 200 °C
|-
|style="background:LightGrey; color:black"|Cool plate temperature
|style="background:WhiteSmoke; color:black" align="center"|
21 °C
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center"|
* 50 mm wafers
* 100 mm wafers
* 150 mm wafers
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center"|
Silicon, III-V, and glass
 
No resist or crystalbond allowed in the HMDS module
|-
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black" align="center"|
1 - 25
|-
|}
 
<br clear="all" />


==Spin Coater: RCD8==
==Spin Coater: RCD8==

Revision as of 15:45, 27 January 2023

Coater Comparison Table

Equipment Spin Coater: Gamma UV Spin Coater: Süss Stepper Spin Coater: Gamma E-beam and UV Spin Coater: RCD8 Spin Coater: LabSpin 02 Spin Coater: LabSpin 03 Spin Coater: Manual All Purpose Spray Coater
Purpose
  • In-line substrate HMDS priming
  • Coating and baking of
    • AZ MiR 701 (29cps)
    • AZ nLOF 2020
    • AZ 5214E
  • Coating and baking of
    • BARC (DUV42S-6)
    • KRF M230Y
    • KRF M35G
    • UVN2300-0.8
  • In-line substrate HMDS priming
  • Coating and baking of
    • AR-P 6200 (CSAR)
    • AZ 5214E
    • AZ MiR 701 (29cps)
    • AZ 4562
  • Edge bead removal on novolac-based resist and SU-8
  • Coating of
    • SU-8
    • AZ 5214E
    • AZ 4562
    • AZ MiR
    • AZ nLOF
  • Edge bead removal
  • Coating of E-beam resists
    • CSAR, ZEP, PMMA/MMA, HSQ(FOx)
  • Coating of UV resists
    • AZ5214E, AZ4562, AZMiR701, AZnLOF, SU-8
  • Coating of imprint resists
  • Coating of
    • ESPACER
    • Experimental resists
  • Coating on
    • Experimental substrates
  • Spraying imprint resist
  • Spraying photoresist
  • Spraying of other solutions
Performance Substrate handling
  • Cassette-to-cassette
  • Vacuum handling and detection
  • Vacuum spin chuck
  • Cassette-to-cassette
  • Vacuum handling and detection
  • Vacuum spin chuck
  • Cassette-to-cassette
  • Vacuum handling and detection
  • Vacuum spin chuck
  • Single substrate
  • Vacuum chuck for 4" and 6"
  • 4" non-vacuum chuck for fragile substrates
  • Single substrate
  • Vacuum chucks for chips, 2", 4", and 6"
  • 4" edge handling chuck
  • Single substrate
  • Vacuum chuck
  • Can handle almost any sample size and shape
Permanent media
  • AZ MiR 701 (29cps) resist
  • AZ nLOF 2020 resist
  • AZ 5214E resist
  • PGMEA solvent for backside rinse and spinner bowl cleaning
  • DUV42S-6 (BARC)
  • KRF M230Y resist
  • KRF M35G resist
  • AR-P 6200.09 (CSAR) for 2", 4", and 6"
  • AZ5214E for 2", 4", and 6"
  • AZ MiR 701 (29cps) for 4", and 6"
  • AZ4562 for 4", and 6"
  • PGMEA solvent for edge bead removal, backside rinse, and spinner bowl cleaning
  • No permanent media
Only manual dispense Only manual dispense
  • No permanent media
Manual dispense option
  • no manual dispense
  • syringe dispense (60cc) of PGMEA-based resist
  • no manual dispense
  • syringe dispense (60cc) of PGMEA and anisole-based resist
  • no manual dispense
  • syringe dispense (30cc) of PGMEA and anisole-based resist (2" only)
  • yes
  • pneumatic dispense for SU-8 resist and EBR solvent
  • Two syringe pumps
Process parameter range Spindle speed
  • 10 - 6000 rpm
  • 10 - 6000 rpm
  • 10 - 6000 rpm
  • 10 - 5000 rpm (3000 rpm with non-vacuum chuck)
  • 100 - 5000 rpm (3000 rpm with edge handling chuck)
  • 100 - 7000 rpm
Gyrset
  • no
  • no
  • no
  • optional (max. speed 3000 rpm)
  • no
  • no
Substrates Substrate size
  • 50 mm wafers (tool change required)
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers (tool change required)
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers (may require tool change)
  • 2" or 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 100 mm wafer
  • 150 mm wafer
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafer
  • small pieces down to 10x10 mm2
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafer
  • small pieces down to 3x3 mm2
  • Any sample(s) that fit inside machine
Batch size
  • 1 - 25
  • 1 - 25
  • 1 - 25
  • 1
  • 1
  • 1
  • 1
Allowed materials
  • Silicon
  • Glass

No resist or crystalbond allowed in the HMDS module

  • Silicon
  • Glass
  • Silicon
  • III-V materials
  • Glass

No resist or crystalbond allowed in the HMDS module

  • All cleanroom materials except III-V materials
  • Silicon
  • III-V materials
  • Glass
  • All cleanroom materials
  • All chemicals to be spray coated must be approved specifically for spray coating
  • Any non-toxic, non-particulate and non-crosslinking material is likely to be approved


Spin coating

The process of spin coating consists of a selection of the following steps:

  • Priming (typically HMDS)
  • Acceleration to a low spin speed if dynamic dispense is used
  • Resist dispense (static or dynamic)
  • Resist spreading at low spin speed
  • Spin-off
  • Backside rinse (typically during spin-off)
  • Edge-bead removal
  • Softbake (contact or proximity)


After priming, the wafer is centered on the coater chuck and held in place by vacuum, or in some cases pins. If static dispense is used, the wafer remains static during the ensuing resist dispense. In the case of dynamic dispense, the wafer rotates at low spin speed during the dispense. Using too high spin speed during dispense can cause surface wetting issues, while a too low spin speed causes the resist to flow onto the backside of the wafer. After dispense, a short spin at low spin speed may be used in order to spread the resist over the wafer surface before spin-off.

Spin-off

The spin-off cycle determines the thickness of the resist coating. For a given resist, the thickness is primarily a function of the spin-off speed and the spin-off time, both following an inverse power-law (y=k*x^-a). The acceleration to the spin-off speed also influences the thickness, but the effect is dependent on previous steps. The spin-off is usually a simple spin at one speed, but it may be comprised of several steps at different spin speeds. After spin-off, the wafer is decelerated.

The coated thickness, t, as a function of the spin-off speed, w, follows an inverse power-law, t = k * w-a. The constant, k, is a function of the resist viscosity and solid content, and the spin-off time. The exponent, a, is dependent on solvent evaporation, and is typically ~½ for UV resists. This means that from the thickness t1 achieved at spin speed w1, one can estimate the spin speed w2 needed to achieve thickness t2 using the relation:
t1*w1½ = t2*w2½ => w2 = w1 * t12/t22.
For thick SU-8, however, a is observed to be ~1 (probably due to the low solvent content and/or the formation of skin). In this case, the relation simply becomes:
t1*w1 = t2*w2 => w2 = w1 * t1/t2.

Backside rinse

Dependent on the spin speeds used in the various steps of the spin coating, resist may creep over the edge of the wafer and onto the backside. Also, some resists tend to leave fine strings of resist protruding from the edge of the wafer, or folded onto the backside, an effect sometimes referred to as "cotton candy". This resist will contaminate the softbake hotplate, and thus subsequent wafers with resist. In a backside rinse step, solvent administered through a nozzle to the backside of the wafer while spinning at low or medium spin speed dissolves the resist and washes it away. After the rinse, a short spin at medium spin speed dries the wafer before the softbake. During the backside rinse solvent inevitably creeps onto the front side of the wafer. This effect may be used to dissolve and subsequently remove an edge-bead, but it may also leave the rim of the wafer exposed. As an alternative to backside rinse, a wafer which is left dirty on the backside by the spin coat process may be softbaked in proximity in order to protect the hotplate from contamination. This leaves front side coating intact, but also leaves the backside dirty.

Edge bead

During spin coating, resist builds up at the edge of the wafer due to the change in surface tension at the edge. This phenomenon is called an edge-bead. Dependent on spin coating parameters, the coating may be several times thicker at the edge than in the central area. In a subsequent hard contact exposure step, this edge-bead induces an undesired proximity gap which reduces the lateral resolution, and may even cause the wafer to stick to the mask.

In an edge-bead removal step, solvent administered through a nozzle positioned at the edge of the wafer while spinning at low or medium spin speed dissolves the resist and washes it away. After the removal, a short spin at medium spin speed dries the wafer before the softbake. Dependent on the viscosity (solvent content) of the resist at the point of edge-bead removal, this drying spin may cause the resist to re-flow and create a secondary edge-bead. In some cases, it may be necessary to (partially) softbake the resist before edge-bead removal.

Softbake

After spin coating, the solvent in the resist formulation must be evaporated in a baking step in order to solidify the resist. This softbake can be carried out as a contact bake or a proximity bake. In a contact bake, the wafer is held in close contact to the hotplate surface while resting on shallow bumps only 150µm above the hotplate. In a proximity bake, the wafer is first moved into proximity, e.g. 1mm, of the hotplate surface, then held there (on the lift pins) for the duration of the bake.

Spin coaters at DTU Nanolab

Spin Coater: Gamma UV

Spin Coater: Gamma UV in E-5

Spin Coater: Gamma UV was installed at DTU Nanolab in March 2015. It is a Gamma 2M cluster from Süss MicroTec with spin coating, HMDS vapour priming, and baking modules.

The system handles 4" and 6" wafers without size conversion, and can be set up to handle 2" or 8".

The coater is equipped with 3 different resist lines, as well as 1 syringe line:

  • AZ MiR 701
  • AZ nLOF 2020
  • AZ 5214E
  • Syringe, which can be used for various resists

The processes that are available on the system are developed by Nanolab. Upon request, it is possible to establish new processes. Use of the syringe requires special training, and would as a starting point require batches in excess of 20 wafers.

Training video

The user manual, quality control procedures and results, user APVs, and contact information can be found in LabManager - requires login

Process information

Equipment performance and process related parameters

Purpose
  • HMDS priming
  • Spin coating of PGMEA based UV resists
  • Spin coating of E-beam resists 1)
  • Soft baking
Resist
  • AZ MiR 701 (29cps)
  • AZ nLOF 2020
  • AZ 5214E
  • 60cc syringe dispense
Performance HMDS contact angle

  60 - 80°

Coating thickness
  • AZ MiR 701: 1.5-4 µm
  • AZ nLOF 2020: 1.5-5 µm
  • AZ 5214E: 1.5-5 µm
  • AZ 4562: 5-15 µm
Process parameters Priming temperature

  120 °C

Spin speed

  10 - 6000 rpm

Spin acceleration

  10 - 10000 rpm/s

Hotplate temperature

  25 - 200 °C

Cool plate temperature

  21 °C

Substrates Substrate size
  • 50 mm wafers 1)
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers 1)
Allowed materials

Silicon and glass

Resists and crystalbond are not allowed in the HMDS module

Batch

  1 - 25

1) Requires tool change.

Spin Coater: Gamma E-beam and UV

Spin Coater: Gamma E-beam & UV in E-5

Spin Coater: Gamma E-beam and UV was installed at DTU Nanolab in June 2017. It is a Gamma 4M cluster from Süss MicroTec with spin coating, HMDS vapour priming, and baking modules. The system handles 2", 4", and 6" wafers without size conversion, using two separate coater stations.

The 2" coater station is equipped with 1 resist line, as well as 1 syringe line:

  • AR-P 6200.09 (CSAR)
  • Syringe, which can be used for various resists (anisole-based or PGMEA-based). We currently recommend against using the syringe, as the process setup is quite demanding. Use a manual spin coater instead.


The 4"/6" coater station is equipped with 4 different resists lines:

  • AZ 5214E
  • AZ MiR 701
  • AR-P 6200.09 (CSAR)
  • AZ 4562

The processes that are available on the system are developed by Nanolab. Upon request, it is possible to establish new processes. Use of the syringe requires special training, and requires batch processing - it is not for processing a few wafers now and then.

Training video

The user manual, quality control procedures and results, user APVs, and contact information can be found in LabManager - requires login

Process information

Equipment performance and process related parameters

Purpose
  • HMDS priming
  • Spin coating of anisole based E-beam resists
  • Spin coating of PGMEA based UV resists
  • Soft baking
  • Edge bead removal (CSAR and novolac-based UV resists)
Resist
  • AR-P 6200.09 (CSAR)
  • AZ 5214E
  • AZ MiR 701 (29cps)
  • AZ 4562
  • 30cc syringe dispense
Performance HMDS contact angle

  60 - 80° (on Silicon)

Coating thickness
  • AR-P 6200.09 (CSAR): 170-500 nm
  • AZ 5214E: 1.5-5 µm
  • AZ MiR 701: 1.5-4 µm
  • AZ 4562: 5-25 µm
Process parameters Priming temperature

  120 °C

Spin speed

  10 - 6000 rpm

Spin acceleration

  10 - 10000 rpm/s

Hotplate temperature

  25 - 200 °C

Cool plate temperature

  21 °C

Substrates Substrate size
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
Allowed materials

  Silicon, III-V, and glass

  Resists and crystalbond are not allowed in the HMDS module

Batch

  1 - 25


Spin Coater: RCD8

Spin coater: RCD8 is located in C-1

Feedback to this section: click here

Coater comparison table

Spin Coater: RCD8 is a model RCD8 T spin coater from Süss MicroTec with a motorized media arm and Gyrset functionality. It's primary purpose is spin coating of SU-8 resist. However, due to the possibility of using a non-vacuum chuck, the spin coater is also suitable for coating of substrates with e.g. textured backsides or membranes.

The user manual, user APV, and contact information can be found in LabManager

Process information

Spin coating

Automatic dispense

Recipes and templates

Processing results

Equipment performance and process related parameters

Purpose
  • Spin coating of SU-8 resists
  • Spin coating of PGMEA based AZ resists
  • Spin coating of wafers with structured backside
  • Edge bead removal
Resist
  • manual dispense
  • automatic dispense from syringe
Performance Coating thickness
  • SU-8 resits: 0.1-200+ µm
  • AZ 5214E: 1.5-3 µm
  • AZ 4562: 8-15 µm
  • AZ MiR 701: 1.5-3 µm
  • AZ nLOF 2020: 2-3.5 µm
Process parameters Spin speed

Vacuum chuck: 10 - 5000 rpm
Non-vacuum chuck: Max. 3000 rpm

Spin acceleration

10 - 3000 rpm/s
Max. 1500 rpm/s with Gyrset

Substrates Substrate size
  • 100 mm wafers
  • 150 mm wafers (vacuum chuck only)
Allowed materials

All cleanroom materials ?

Batch

1


Manual Spin Coaters

Go back to Coater comparison table.

Labspin 2.JPG Labspin 3 + fumehood 11.JPG IMG 1175.JPG


Spin Coater: Labspin 02 Spin Coater: Labspin 03 + fumehood 11 Spin Coater: Manual All Purpose (Decommissioned)
Loacted in wetbench 08 in E-5 Located in wetbench 09 in E-5 Located in fumehood in C-1
LabSpin 6, Süss MicroTec LabSpin 6, Süss MicroTec WS-650, Laurell
LabManager LabManager LabManager


Training video: LabSpin02 + 03

Process information

Spin curves (LabSpin 6): AZ 5214E‎, AZ nLOF 2020, ZEP 520A‎, FOX-15, AZ 4562‎, CSAR 6200, AZ MiR 701.

More information on resists (incl. spin curves) is available in the Resist Overview.


This table is under construction Section under construction.jpg

Available bowlsets:

Component solvent Cleaning solvent List of resists Comments
AZ resist PGMEA/Ethyl Lactate Acetone AZ 5214E, AZ 4562, AZ MiR 701, AZ nLOF 2000 series,

mr-I8100R?

Two sets available
CSAR/ZEP/mrEBL/PMMA Anisole Remover 1165 AR-P 6200 series (CSAR 62), ZEP520A, mr EBL 6000, PMMA (in anisole),

UV5?, mr-T85L?, XNIL26?, mri8000?, mr-I 7010E?, mr-XNIL26_SF?, mrNIL210?

HSQ/AR-N 8200 MIBK/PGMEA Acetone HSQ (FOx series), AR-N 8200
OrmoComp/OrmoStamp Propyl Acetate Acetone OrmoComp, OrmoStamp, OrmoPrime, OrmoClad?

Inkron?, mr-I-7030R?, mr-I 8020E?, mr-I-7010E?, mrNIL210?, mr-I 8500E?, mr-T85?, MRT HI01XP?, Protek B3?, mrUVCur21?, mr-I 8100E_XP?, mrNIL210?, MRT HI01XP?, mr-NIL 6000.3E?, mr-I 8100R_XP?

BCB/CYCLOTENE Mesitylene T1100 3022-X, 4022-X
Epoxy/Acrylate Cyclopentanone/PGMEA Acetone SU-8 2000 series, mr-DWL, LOR (1A, 3A, 5A)

mr-i 8030e?, mr-NIL200?, DELO-PRE/OM4310?, OrmoStamp?, Inkron?, mr-I 8020E?, OM4310?

AR-P 617/AR-N 7520 PGME/PGMEA Acetone AR-N 7500 series
Polymer Ps-b-PDMS/block copolymer Heptane Ethyl Acetate
DIRTY bowlset Anything Organic Use the appropriate cleaning reagent for your resist


Equipment performance and process related parameters

Purpose Labspin

Spin coating of resist ONLY in dedicated bowlsets

Please do NOT use substances which is not for the dedicated bowlsets

All purpose

Spin coating of dirty substances in All purpose

Process parameters Spin speed
  • Vacuum chuck: 100 - 5000 rpm
  • Edge handling chuck: Max. 3000 rpm
Spin acceleration
  • 200 - 4000 rpm/s
Substrates Substrate size
  • Chips 5x5 mm and up
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
Allowed materials

All cleanroom materials

Please ONLY use substances which is for the dedicated bowlsets in labspins

Batch

1


Spray Coater

Spray Coater in Cleanroom C-1

The spray coater at DTU Nanolab is located in Cleanroom C-1. The machine is an ExactaCoat from Sono-tek which can be fitted with one of three different nozzles depending on the nature of the spray coating tasks at hand. The three different nozzles (Impact, AccuMist and Vortex) are optimized for different applications such as spray coating of large areas (e.g. entire wafers), smaller areas (e.g. wafer pieces or other small samples) or already structured samples that cannot be coated uniformly by spin coating. All nozzles use an ultrasonic tranducer for atomizing the solution to be spray coated. It is therefore a prerequisite that all components are compatible with this process. This is the case with most substances, although process parameters may need optimization to give satisfactory results.

Practically any sample that will fit inside the spray coater can be processed. Spray patterns are easily programmed either using predefined spray patterns (1D line, 2D rectangles/circles/meanders/spirals) or custom 3D spray patterns.

The spray coating process as well as major features of the three nozzles are described into more detail in the manual which can be found via the Equipment Info page in LabManager under the Documents sections. The manual can also be found by clicking this direct link.

Further information about the spray coater (manual, process log, technical information etc.) can be found in LabManger:

Spray coater in LabManager

Process development

Equipment performance and process related parameters

Equipment Spray Coater
Purpose
  • Spraying imprint resists (primarily mr-NIL 6000E and mr-I 8000E)
  • Spraying photoresist (primarily AZ-4562)
  • Spraying of other solutions
Performance Substrate handling
  • Can handle almost any sample size and shape (although no automatic handling)
Permanent media
  • No permanent media
Manual dispense option
  • Two syringe pumps
Process parameter range Solution viscosity
  • Should not exceed 20 cP
Chemical properties
  • Must be non-toxic
  • Must be compatible with titanium
  • Resistant to ultrasonic sonication
Substrates Batch size
  • Any sample(s) size and number that fit inside machine
Allowed materials
  • All chemicals to be spray coated must be approved specifically for spray coating
  • Most non-toxic, non-particulate and non-crosslinking material likely to be approved
  • Suspensions challenging due to very low diameter tubing