Tests performed with UV resist:
The tests were performed on a 100mm wafer patterned on MLA3, with 2.2um AZ5214E resist.
Tests performed with DUV resist:
The resist used was a negative DUV resist (UVN) with 915nm + 88nm BARC layer.
SiO2 test - 5 jan 2024
- The SiO2 layer deposited was 2um, deposited on the C1 furnace (recipe: WET1100, 12h40+00:20).
- They were patterned with 915 UVN resist (DUV negative) and 65nm of BARC.
- The following results were processed on chips (2*2cm) bonded to a 100mm dummy wafer.
Etch test of Silicon Nitride
- The nitride layer deposited was 560nm, on the PECVD4 (recipe: Standard HF SiN with wafer clean, for 1h).
- They were patterned with 750 DUV resist and 65nm of BARC (exposure:355 J/m2, focus:-3.1).
- The following results were processed on chips (2*2cm) bonded to a 100mm dummy wafer.