==Deposition of Silicon Nitride using LPCVD== | ==Deposition of Silicon Nitride using LPCVD== | ||
LPCVD silicon nitride can be | LPCVD silicon nitride can be deposited in an [[Specific Process Knowledge/Thin film deposition/B2 Furnace LPCVD Nitride|LPCVD nitride furnace]]. Danchip has two LPCVD nitride furnaces: A new furnace for deposition of stoichiometric nitride on 4" or on 6" wafers and an older furnace for deposition of stoichiometric nitride and low stress nitride on 4" wafers. | ||
The LPCVD nitride deposition is a batch process, meaning that you can run a batch of 25-35 wafers at a time. The deposition takes place at temperatures of 780-850 degrees Celsius. The LPCVD silicon nitride has a good step coverage, and the film thickness is very uniform over the wafers. On the furnaces we have standard processes for deposition of stoichiometric nitride (Si<sub>3</sub>N<sub>4</sub>) and for deposition of low stress nitride (SNR). | The LPCVD nitride deposition is a batch process, meaning that you can run a batch of up to 25-35 wafers at a time. The deposition takes place at temperatures of 780-850 degrees Celsius, and at a pressure of 200-230 mTorr. The LPCVD silicon nitride has a good step coverage, and the film thickness is very uniform over the wafers. On the furnaces we have standard processes for deposition of stoichiometric nitride (Si<sub>3</sub>N<sub>4</sub>) and for deposition of low stress nitride (SNR). | ||
*[[/Deposition of Silicon Nitride using LPCVD|Deposition of | *[[/Deposition of Silicon Nitride using LPCVD|Deposition of Silicon Nitride using LPCVD]] | ||
==Deposition of Silicon Nitride using PECVD== | ==Deposition of Silicon Nitride using PECVD== | ||
PECVD nitride and oxynitride can be deposited in one of the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] systems. You can run 1-3 wafers at a time depending on which one of the PECVD's you use. The deposition takes place at 300 degrees | PECVD nitride and oxynitride can be deposited in one of the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] systems at Danchip. You can run 1-3 wafers at a time depending on which one of the PECVD's you use. The deposition takes place at 300 degrees Celsius. This can be of importance for some applications, but it gives a less dense film compared to LPCVD nitride, and the stoichiometry is on the following form: Si<sub>x</sub>N<sub>y</sub>O<sub>z</sub>H<sub>v</sub>. The step coverage and the thickness uniformity of the film are not as good as for the LPCVD nitride. In one of our PECVD systems (PECVD3) we allow small amounts of metal on the wafers entering the system; this is not allowed in the LPCVD furnace and in the clean PECVD (PECVD1). We also have a PECVD for deposition on III-V materials (PECVD2). | ||
*[[/Deposition of Silicon Nitride using PECVD|Deposition of | *[[/Deposition of Silicon Nitride using PECVD|Deposition of Silicon Nitride using PECVD]] - ''or oxynitride'' | ||
==Comparison of LPCVD and PECVD for silicon nitride deposition== | ==Comparison of LPCVD and PECVD for silicon nitride deposition== | ||
Line 27: | Line 27: | ||
*Si<sub>x</sub>N<sub>y</sub>H<sub>z</sub> | *Si<sub>x</sub>N<sub>y</sub>H<sub>z</sub> | ||
*Si<sub>x</sub>O<sub>y</sub>N<sub>z</sub>H<sub>v</sub> | *Si<sub>x</sub>O<sub>y</sub>N<sub>z</sub>H<sub>v</sub> | ||
Silicon nitride can be doped with boron, phosphorus or germanium | |||
|- | |- | ||
|Film thickness | |Film thickness | ||
Line 33: | Line 33: | ||
*Si<sub>3</sub>N<sub>4</sub>: ~50 Å - ~3000 Å | *Si<sub>3</sub>N<sub>4</sub>: ~50 Å - ~3000 Å | ||
*SRN: ~50 Å - ~10000 Å | *SRN: ~50 Å - ~10000 Å | ||
Thick nitride layers | Thick nitride layers have to be deposited over more runs | ||
| | | | ||
*~40 nm - 10 µm | *~40 nm - 10 µm | ||
Line 59: | Line 59: | ||
|Batch size | |Batch size | ||
| | | | ||
*Deposition on both sides of the substrate | *Deposition on both sides of the substrate | ||
Old nitride furnace: | |||
*1-35 4" wafers per run (dependent on size of quarz boat) | |||
New nitride furnace: | |||
*1-25 4" or 6" wafers per run | |||
| | | | ||
*Deposition on one side of the substrate | |||
*1-3 4" wafers or one 6" wafer or many smaller chips per run | *1-3 4" wafers or one 6" wafer or many smaller chips per run | ||
|- | |- | ||
| Substrate materials allowed | | Substrate materials allowed | ||
| | | | ||
* | *Silicon wafers (new wafers from a new box or RCA cleaned wafers) | ||
**with layers of silicon oxide or silicon (oxy)nitride | **with layers of silicon oxide or silicon (oxy)nitride (RCA cleaned) | ||
*Quartz wafers | **from furnace in stack A or B in cleanroom 2 | ||
*Quartz wafers (RCA cleaned) | |||
| | | | ||
*Silicon wafers | *Silicon wafers | ||
**with layers of silicon oxide or silicon (oxy)nitride | **with layers of silicon oxide or silicon (oxy)nitride | ||
*Quartz | *Quartz wafers | ||
*Small amount of metal < 5% of the wafer coverage (ONLY in PECVD3!) | *Small amount of metal < 5% of the wafer coverage (ONLY in PECVD3!) | ||
|- | |- |
Revision as of 09:03, 18 December 2008
Deposition of Silicon Nitride can be done with either LPCVD (Low Pressure Chemical Vapor Deposition) or PECVD (Plasma Enhanced Chemical Vapor Deposition).
Deposition of Silicon Nitride using LPCVD
LPCVD silicon nitride can be deposited in an LPCVD nitride furnace. Danchip has two LPCVD nitride furnaces: A new furnace for deposition of stoichiometric nitride on 4" or on 6" wafers and an older furnace for deposition of stoichiometric nitride and low stress nitride on 4" wafers.
The LPCVD nitride deposition is a batch process, meaning that you can run a batch of up to 25-35 wafers at a time. The deposition takes place at temperatures of 780-850 degrees Celsius, and at a pressure of 200-230 mTorr. The LPCVD silicon nitride has a good step coverage, and the film thickness is very uniform over the wafers. On the furnaces we have standard processes for deposition of stoichiometric nitride (Si3N4) and for deposition of low stress nitride (SNR).
Deposition of Silicon Nitride using PECVD
PECVD nitride and oxynitride can be deposited in one of the PECVD systems at Danchip. You can run 1-3 wafers at a time depending on which one of the PECVD's you use. The deposition takes place at 300 degrees Celsius. This can be of importance for some applications, but it gives a less dense film compared to LPCVD nitride, and the stoichiometry is on the following form: SixNyOzHv. The step coverage and the thickness uniformity of the film are not as good as for the LPCVD nitride. In one of our PECVD systems (PECVD3) we allow small amounts of metal on the wafers entering the system; this is not allowed in the LPCVD furnace and in the clean PECVD (PECVD1). We also have a PECVD for deposition on III-V materials (PECVD2).
- Deposition of Silicon Nitride using PECVD - or oxynitride
Comparison of LPCVD and PECVD for silicon nitride deposition
LPCVD | PECVD | |
---|---|---|
Stoichiometry |
Si3N4: Stoichiometric nitride SRN: Silicon rich nitride (low stress nitride) |
Silicon nitride can be doped with boron, phosphorus or germanium |
Film thickness |
Thick nitride layers have to be deposited over more runs |
|
Process Temperature |
|
|
Step coverage |
|
|
Film quality |
|
|
Batch size |
Old nitride furnace:
New nitride furnace:
|
|
Substrate materials allowed |
|
|
Etch rate in 80 oC KOH | Expected <1 Å/min | Dependent on recipe: ~1-10 Å/min |
Etch rate in BHF | Very low | Very high compared to the etch rate of LPCVD nitride |