Specific Process Knowledge/Lithography/Coaters: Difference between revisions
Line 9: | Line 9: | ||
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment | !colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment | ||
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Coaters#Spin Track 1 + 2|Spin Coater: Gamma UV]]</b> | |||
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Coaters#Spin Track 1 + 2|Spin Track 1 + 2]]</b> | |style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Coaters#Spin Track 1 + 2|Spin Track 1 + 2]]</b> | ||
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Coaters#SSE Spinner|SSE Spinner]]</b> | |style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Coaters#SSE Spinner|SSE Spinner]]</b> | ||
Line 18: | Line 19: | ||
|- | |- | ||
!style="background:silver; width:100px; color:black;" align="center"|Purpose | !style="background:silver; width:100px; color:black;" align="center"|Purpose | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
|style="background:WhiteSmoke; color:black"| | |||
*In-line substrate HMDS priming | |||
*Coating and baking of | |||
**AZ MiR 701 (29cps) resist | |||
**AZ nLOF 2020 resist | |||
**AZ 5214E | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*In-line substrate HMDS priming | *In-line substrate HMDS priming | ||
Line 67: | Line 74: | ||
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Performance | !style="background:silver; color:black" align="center" valign="center" rowspan="3"|Performance | ||
|style="background:LightGrey; color:black"|Substrate handling | |style="background:LightGrey; color:black"|Substrate handling | ||
|style="background:WhiteSmoke; color:black"| | |||
* Cassette-to-cassette | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* Cassette-to-cassette | * Cassette-to-cassette | ||
Line 83: | Line 92: | ||
|- | |- | ||
|style="background:LightGrey; color:black"|Permanent media | |style="background:LightGrey; color:black"|Permanent media | ||
|style="background:WhiteSmoke; color:black"| | |||
* AZ MiR 701 (29cps) resist | |||
* AZ nLOF 2020 resist | |||
* AZ 5214E resist | |||
* PGMEA solvent for backside rinse and spinner bowl cleaning | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* AZ MiR 701 (29cps) resist | * AZ MiR 701 (29cps) resist | ||
Line 101: | Line 115: | ||
|- | |- | ||
|style="background:LightGrey; color:black"|Manual dispense option | |style="background:LightGrey; color:black"|Manual dispense option | ||
|style="background:WhiteSmoke; color:black"| | |||
* syringe dispense | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* no | * no | ||
Line 114: | Line 130: | ||
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Process parameter range | !style="background:silver; color:black" align="center" valign="center" rowspan="2"|Process parameter range | ||
|style="background:LightGrey; color:black"|Spindle speed | |style="background:LightGrey; color:black"|Spindle speed | ||
|style="background:WhiteSmoke; color:black"| | |||
*10 - 6000 rpm | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*10 - 9990 rpm | *10 - 9990 rpm | ||
Line 129: | Line 147: | ||
|- | |- | ||
|style="background:LightGrey; color:black"|Gyrset | |style="background:LightGrey; color:black"|Gyrset | ||
|style="background:WhiteSmoke; color:black"| | |||
*no | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*no | *no | ||
Line 145: | Line 165: | ||
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates | !style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates | ||
|style="background:LightGrey; color:black"|Substrate size | |style="background:LightGrey; color:black"|Substrate size | ||
|style="background:WhiteSmoke; color:black"| | |||
*50 mm wafers (tool change required) | |||
*100 mm wafers | |||
*150 mm wafers | |||
*200 mm wafers (tool change required) | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*100 mm wafers | *100 mm wafers | ||
Line 174: | Line 199: | ||
|- | |- | ||
|style="background:LightGrey; color:black"|Batch size | |style="background:LightGrey; color:black"|Batch size | ||
|style="background:WhiteSmoke; color:black"| | |||
*1 - 25 | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*1 - 25 | *1 - 25 | ||
Line 190: | Line 217: | ||
|- | |- | ||
| style="background:LightGrey; color:black"|Allowed materials | | style="background:LightGrey; color:black"|Allowed materials | ||
|style="background:WhiteSmoke; color:black"| | |||
*Silicon | |||
*Glass | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*Silicon | *Silicon |
Revision as of 11:06, 15 January 2016
Coaters: Comparison Table
Equipment | Spin Coater: Gamma UV | Spin Track 1 + 2 | SSE Spinner | Spin Coater: RCD8 | Spin Coater: Manual All Resists | Spin Coater: Manual Standard Resists | Spin Coater: Manual All Purpose | Spray Coater | |
---|---|---|---|---|---|---|---|---|---|
Purpose |
|
|
|
|
|
|
|
| |
Performance | Substrate handling |
|
|
|
|
|
Single substrate |
| |
Permanent media |
|
|
|
|
Only manual dispense |
| |||
Manual dispense option |
|
|
|
|
| ||||
Process parameter range | Spindle speed |
|
|
|
|
|
|
|
|
Gyrset |
|
|
|
|
|
|
|
||
Substrates | Substrate size |
|
|
|
|
|
|
|
|
Batch size |
|
|
|
|
|
|
|
| |
Allowed materials |
|
|
|
|
|
|
|
|
SSE Spinner
Feedback to this section: click here
SSE Spinner, Maximus 804, SSE Sister Semiconductor Equipment is a resist spinning system at Danchip which can be used for spinning on 2", 4" and 6" substrates.
The system is equipped with 2 different resists lines:
- AZ 5214E
- AZ 4562
and
- 2 syringe lines, which can be used for spinning of e-beam resist.
The user manual, user APV, and contact information can be found in LabManager
Process information
The typical flow for resist spinning is divided in 3 steps: video, spinning and soft bake. You need to create a separate recipe for each station and then collect the recipes in a flow. For the video station we have 3 standard recipes for 3 different wafer sizes: 2inch, 4inch, 6inch. To create a recipe for the coater station you need to describe spinning sequence using the predefined functions. Then you create recipe for the hotplates. After all recipes are created they can be set together in the different flows. It is why we are not recommending the user just change some parameters in the recipe, this change can effect some other flows.
Flow names, process parameters, and test results:
- _DCH_100mm_AZ5214E_1,5um
Spin-off: 10 s at 2300 rpm closed followed by 10s at 3500 rpm open.
Soft bake: 90 s at 90°C in contact
Substrate | Thickness | Uniformity (+/-) | Test date | Tester initials | Comments |
---|---|---|---|---|---|
Silicon with native oxide | 1,367 | 3,1% | 10/7 2015 | chasil | with HMDS. Average of 3 wafers
|
Silicon with native oxide | 1,409 | 2,4% | 12/15 2015 | chasil | with HMDS. Average of 3 wafers |
- _DCH_100mm_AZ5214E_2,2um
Spin-off: 40 s at 2200 rpm open.
Soft bake: 60 s at 90°C in contact
- _DCH_100mm_AZ5214E_1,5um
Spin-off: 60 s at 725 rpm open with exhaust closed followed by 10s at 3500 rpm open.
Soft bake: 90 s at 95°C in 1 mm proximity
Purpose |
| ||
---|---|---|---|
Resist |
| ||
Performance | Coating thickness |
| |
Process parameters | Spin speed |
100 - 5000 rpm | |
Spin acceleration |
100 - 10000 rpm/s | ||
Hotplate temperature |
| ||
Substrates | Substrate size |
| |
Allowed materials |
All cleanroom materials except III-V materials | ||
Batch |
1 - 24 |
Spin Track 1 + 2
Feedback to this section: click here
Spin Track 1 + 2 is an SVG 88 series track system from Rite Track. Each track consists of a HMDS priming module, a spin coating module, and a baking module. In fact, the only difference between the two tracks is the resist used in the spin coating module. Spin Track 1 + 2 is capable of handling 150 mm wafers, as well as 100 mm wafers, but is currently set up for 100 mm wafer processing.
The Spin Track 1 + 2 is controlled using the Recipe Manager software via the touchscreen on the arm attached to the lefthand end of the track. Recipes for the individual modules are developed by Danchip and combined into flows. The user selects a flow (specific to track 1 or 2), and the appropriate recipes will be downloaded and executed on the appropriate track. The other track runs an empty process (no wafers needed), and can unfortunately not be used by a second user while the first user is processing.
The user manual, user APV, and contact information can be found in LabManager
Process information
- General Spin Track 1 + 2 process information
- HMDS priming on Spin Track 1 and 2
- AZ MiR 701 (29cps) coating on Spin Track 1
- AZ nLOF 2020 coating on Spin Track 2
- Post-exposure baking on Spin Track 2
Spin Track | 1 | 2 | |
---|---|---|---|
Purpose |
|
| |
Resist |
AZ MiR 701 (29cps) positive tone |
AZ nLOF 2020 negative tone | |
Performance | Coating thickness |
1 - 3 µm |
1 - 4 µm |
HMDS contact angle |
60° - 90°; standard recipe 82° (on SiO2) | ||
Process parameters | Spin speed |
10 - 9990 rpm | |
Spin acceleration |
1000 - 50000 rpm/s | ||
Hotplate temperature |
90°C |
110°C | |
HMDS priming temperature |
50°C | ||
Substrates | Substrate size |
100 mm wafers | |
Allowed materials |
Silicon and glass wafers Film or pattern of all types | ||
Batch |
1 - 25 |
Spin Coater: Gamma UV
Feedback to this section: click here
Spin Coater: Gamma UV was installed at Danchip in March 2015. It is a Gamma 2M cluster from Süss MicroTec with spin coating, vapour priming, and baking modules. The system handles 4" and 6" wafers without size conversion, and can be set up to handle 2" or 8".
The coater is equipped with 3 different resists lines:
- AZ MiR 701
- AZ nLOF 2020
- AZ 5214E
and
- 1 syringe, which can be used for various resists.
The processes that are available on the system are developed by Danchip. Upon request, it is possible to establish new processes. Use of the syringe requires special training, and would as a starting point require batches in excess of 20 wafers.
The user manual, user APV, and contact information can be found in LabManager
Process information
Purpose |
| |
---|---|---|
Resist |
| |
Performance | HMDS contact angle |
60 - 80° |
Coating thickness |
| |
Process parameters | Priming temperature |
25 - 120 °C |
Spin speed |
10 - 7000 rpm | |
Spin acceleration |
10 - 10000 rpm/s | |
Hotplate temperature |
25 - 200 °C | |
Cool plate temperature |
21 °C | |
Substrates | Substrate size |
|
Allowed materials |
Silicon and glass | |
Batch |
1-25 |
1) Requires tool change.
Spin Coater: RCD8
Feedback to this section: click here
Spin Coater: RCD8 is a model RCD8 T spin coater from Süss MicroTec with a motorized media arm and Gyrset functionality. It's primary purpose is spin coating of SU-8 resist. However, due to the possibility of using a non-vacuum chuck, the spin coater can also be used for coating of substrates with e.g. textured backsides or membranes.
The user manual, user APV, and contact information can be found in LabManager
Process information
Purpose |
| |
---|---|---|
Resist |
| |
Performance | Coating thickness |
|
Process parameters | Spin speed |
Vacuum chuck: 10 - 5000 rpm |
Spin acceleration |
10 - 3000 rpm/s | |
Substrates | Substrate size |
|
Allowed materials |
All cleanroom materials ? | |
Batch |
1 |
Manual Spin Coaters
Go back to Coater comparison table.
| ||
Spin Coater: Manual All Resists | Spin Coater: Manual Standard Resists | Spin Coater: Manual All Purpose |
Loacted in fumehood in A-5 | Located in fumehood in E-5 | Located in fumehood in C-1 |
Labspin 6, Süss | Labspin 6, Süss | WS-650, Laurell |
LabManager | LabManager | LabManager |
Spin curves: AZ5214E, AZnLoF 2020, ZEP520A, FOX-15 |