'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Nitride&action=submit click here]''' | ||
<i> Unless otherwise stated, this page is written by <b>DTU Nanolab internal</b></i> | |||
== Deposition of silicon nitride == | == Deposition of silicon nitride == | ||
Deposition of silicon nitride can be done | Deposition of silicon nitride can be done by either LPCVD (Low Pressure Chemical Vapor Deposition) or PECVD (Plasma Enhanced Chemical Vapor Deposition). Stoichiometric nitride or silicon rich (low stress) LPCVD nitride is deposited on a batch of wafers in a LPCVD nitride furnace. PECVD nitride (or oxynitride) is deposited on a few samples at a time in a PECVD system. LPCVD nitride has a good step coverage and a very good uniformity. Using PECVD it is possible to deposit a much lower temperature and a thicker layer of nitride on different types of samples, but the nitride does not cover sidewalls very well. | ||
It is also possible to deposit silicon nitride | It is also possible to deposit silicon nitride and oxynitride by reactive sputtering. | ||
*[[Specific Process Knowledge/Thin film deposition/Furnace LPCVD Nitride/Deposition of stoichiometric nitride using the 4" LPCVD nitride furnace|Deposition of | *[[Specific Process Knowledge/Thin film deposition/Furnace LPCVD Nitride/Deposition of stoichiometric nitride using the 4" LPCVD nitride furnace|Deposition of stoichiometric nitride using the 4" LPCVD nitride furnace]] | ||
*[[Specific Process Knowledge/Thin film deposition/Furnace LPCVD Nitride/Deposition of low stress nitride using the 6" LPCVD nitride furnace|Deposition of low stress | *[[Specific Process Knowledge/Thin film deposition/Furnace LPCVD Nitride/Deposition of low stress nitride using the 6" LPCVD nitride furnace|Deposition of silicon rich (low stress) nitride using the 6" LPCVD nitride furnace]] | ||
*[[/Deposition of Silicon Nitride using PECVD|Nitride deposition using PECVD]] (''or oxynitride'') | *[[/Deposition of Silicon Nitride using PECVD|Nitride deposition using PECVD]] (''or oxynitride'') | ||
Line 14: | Line 16: | ||
*[[/Deposition of silicon nitride using Lesker sputter system|Nitride deposition using Lesker sputter system]] | *[[/Deposition of silicon nitride using Lesker sputter system|Nitride deposition using Lesker sputter system]] | ||
==Comparison of LPCVD, PECVD and | *[[/Deposition of silicon nitride using Sputter-System Metal-Oxide(PC1)|Nitride deposition using Sputter-System Metal-Oxide(PC1)]] | ||
==Comparison of LPCVD, PECVD, and sputter systems for silicon nitride deposition== | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | ||
Line 24: | Line 28: | ||
![[Specific Process Knowledge/Thin film deposition/Furnace LPCVD Nitride|LPCVD]] | ![[Specific Process Knowledge/Thin film deposition/Furnace LPCVD Nitride|LPCVD]] | ||
![[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] | ![[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] | ||
![[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system|Sputter-System Metal-Nitride(PC3) and Sputter-System Metal-Oxide(PC1)]] | |||
![[Specific Process Knowledge/Thin film deposition/Lesker|Lesker sputter system]] | ![[Specific Process Knowledge/Thin film deposition/Lesker|Lesker sputter system]] | ||
|- | |- | ||
Line 30: | Line 35: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Generel description | !Generel description | ||
|Low Pressure Chemical Vapour Deposition (LPCVD furnace process) | | | ||
|Plasma Enhanced Chemical Vapour Deposition (PECVD process) | *Low Pressure Chemical Vapour Deposition (LPCVD furnace process) | ||
|Reactive sputtering | | | ||
*Plasma Enhanced Chemical Vapour Deposition (PECVD process) | |||
| | |||
*Reactive sputtering | |||
*Pulsed DC reactive sputtering | |||
*Reactive HIPIMS (high-power impulse magnetron sputtering) | |||
|*Reactive sputtering | |||
|- | |- | ||
Line 40: | Line 51: | ||
| | | | ||
*Stoichiometric nitride, Si<sub>3</sub>N<sub>4</sub> | *Stoichiometric nitride, Si<sub>3</sub>N<sub>4</sub> | ||
* | *Silicon rich (low stress) nitride, SRN | ||
| | | | ||
*Si<sub>x</sub>N<sub>y</sub>H<sub>z</sub> | *Si<sub>x</sub>N<sub>y</sub>H<sub>z</sub> | ||
*Si<sub>x</sub>O<sub>y</sub>N<sub>z</sub>H<sub>v</sub> | *Si<sub>x</sub>O<sub>y</sub>N<sub>z</sub>H<sub>v</sub> | ||
Silicon nitride can be doped with boron | Silicon nitride can be doped with boron or phosphorus | ||
|Unknown | | | ||
*Si<sub>x</sub>N<sub>y</sub> (Sputter-System Metal-Nitride(PC3)) | |||
*Si<sub>x</sub>O<sub>y</sub>N<sub>z</sub> (Sputter-System Metal-Oxide(PC1)) | |||
Tunable composition | |||
| | |||
*Unknown | |||
|- | |- | ||
Line 52: | Line 68: | ||
!Film thickness | !Film thickness | ||
| | | | ||
* | *Stoichiometric nitride: ~5 nm - ~230 nm | ||
* | *Silicon rich (low stress) nitride: ~5 nm - ~335 nm | ||
Thicker nitride layers can be deposited over more runs | Thicker nitride layers can be deposited over more runs (maximum two) | ||
| | | | ||
*~40 nm - 10 µm | *~40 nm - 10 µm | ||
|limited by process time. | | | ||
Deposition rate | *limited by process time. | ||
*Deposition rate likely faster than Sputter-System (Lesker) | |||
| | |||
*limited by process time. | |||
*Deposition rate ~ 1-5 nm/min | |||
|- | |- | ||
Line 65: | Line 86: | ||
!Process temperature | !Process temperature | ||
| | | | ||
*780 | *Stoichiometric nitride: 780 °C - 800 °C | ||
*Silicon rich (low stress) nitride: 810 °C - 845 °C | |||
| | |||
*300 °C | |||
| | |||
*Up to 600 °C | |||
| | | | ||
* | *Up to 400 °C | ||
|- | |- | ||
Line 78: | Line 103: | ||
| | | | ||
*Less good | *Less good | ||
| | | | ||
*some step coverage possible, especially by HIPIMS | |||
| | |||
*some step coverage possible but amount unknown | |||
|- | |- | ||
Line 92: | Line 120: | ||
*Less dense film | *Less dense film | ||
*Incorporation of hydrogen in the film | *Incorporation of hydrogen in the film | ||
| | |||
*Deposition on one side of the substrate | |||
*Less dense film | |||
*Properties including density tunable (requires process development) | |||
| | | | ||
*Deposition on one side of the substrate | *Deposition on one side of the substrate | ||
*unknown quality | *unknown quality | ||
*likely O-contamination | |||
|- | |- | ||
Line 104: | Line 137: | ||
| | | | ||
*Dependent on recipe: ~1-10 Å/min | *Dependent on recipe: ~1-10 Å/min | ||
|Unknown | | | ||
*Unknown | |||
| | |||
*Unknown | |||
|- | |- | ||
Line 111: | Line 147: | ||
!BHF etch rate | !BHF etch rate | ||
| | | | ||
*Very low | *Very low ([[Specific_Process_Knowledge/Etch/Etching_of_Silicon_Nitride|more info here]]) | ||
( | |||
| | | | ||
*Very high compared the LPCVD nitride | *Very high compared the LPCVD nitride ([[Specific_Process_Knowledge/Etch/Etching_of_Silicon_Nitride|more info here]]) | ||
|Unknown | | | ||
*Unknown | |||
| | |||
*Unknown | |||
|- | |- | ||
Line 122: | Line 160: | ||
!Batch size | !Batch size | ||
| | | | ||
*1-25 100 mm wafers | *1-15 100 mm wafers (4" furnace), 1-25 100 mm wafers (6" furnace) | ||
*1-25 150 mm wafers (only 6" furnace) | *1-25 150 mm wafers (only 6" furnace) | ||
| | | | ||
*Several smaller samples | *Several smaller samples | ||
*1- | *1-7 50 mm wafers | ||
*1 | *1 100 mm wafers | ||
*1 150 mm wafer | *1 150 mm wafer | ||
Depending on what PECVD you use | Depending on what PECVD you use | ||
| | |||
*many smaller samples | |||
*Up to 10*100 mm or 150 mm wafers | |||
| | | | ||
*Several smaller samples | *Several smaller samples | ||
Line 148: | Line 189: | ||
| | | | ||
*Silicon | *Silicon | ||
*Silicon oxide (with boron, phosphorous | *Silicon oxide (with boron, phosphorous) | ||
*Silicon nitrides (with boron, phosphorous | *Silicon nitrides (with boron, phosphorous) | ||
*Pure quartz (fused silica) | *Pure quartz (fused silica) | ||
|Any | *III-V materials (in PECVD4) | ||
*Small amount of metals (in PECVD3) | |||
| | |||
*Almost any as long as they do not outgas and are not very toxic, see cross-contamination sheets | |||
| | |||
*Any | |||
|- | |- | ||
|} | |} | ||
Line 166: | Line 212: | ||
==Deposition of Silicon Nitride using LPCVD== | ==Deposition of Silicon Nitride using LPCVD== | ||
LPCVD silicon nitride can be deposited in a [[Specific Process Knowledge/Thin film deposition/B2 Furnace LPCVD Nitride|LPCVD nitride furnace]]. | LPCVD silicon nitride can be deposited in a [[Specific Process Knowledge/Thin film deposition/B2 Furnace LPCVD Nitride|LPCVD nitride furnace]]. DTU Nanolab has two LPCVD nitride furnaces: A new furnace (installed in 2008) for deposition of stoichiometric nitride on 4" or on 6" wafers and an older furnace (installed in 1995) for deposition of stoichiometric nitride and low stress nitride on 4" wafers. | ||
The LPCVD nitride deposition is a batch process, meaning that nitride can be deposited on a batch of up to 15 wafers (in the old nitride furnace) or 25 wafers (in the new nitride furnace) at a time. The deposition takes place at temperatures of 780-845 degrees Celsius and at a pressure of 120-200 mTorr. The LPCVD silicon nitride has a good step coverage, and the film thickness is very uniform over the wafers. On the furnaces there are standard processes for deposition of stoichiometric nitride (Si<sub>3</sub>N<sub>4</sub>) and for deposition of low stress nitride (SRN) (only on the old nitride | The LPCVD nitride deposition is a batch process, meaning that nitride can be deposited on a batch of up to 15 wafers (in the old nitride furnace) or 25 wafers (in the new nitride furnace) at a time. The deposition takes place at temperatures of 780-845 degrees Celsius and at a pressure of 120-200 mTorr. The LPCVD silicon nitride has a good step coverage, and the film thickness is very uniform over the wafers. On the furnaces there are standard processes for deposition of stoichiometric nitride (Si<sub>3</sub>N<sub>4</sub>) and for deposition of low stress nitride (SRN) (only on the old nitride furnace). | ||
*[[/Deposition of Silicon Nitride using LPCVD|Deposition of Silicon Nitride using LPCVD]] | *[[/Deposition of Silicon Nitride using LPCVD|Deposition of Silicon Nitride using LPCVD]] | ||
==Deposition of Silicon Nitride using PECVD== | ==Deposition of Silicon Nitride using PECVD== | ||
PECVD nitride and oxynitride can be deposited in one of the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] systems at | PECVD nitride and oxynitride can be deposited in one of the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] systems at DTU Nanolab. You can run 1-3 wafers on several smaller chips at a time depending on which one of the PECVD's you use. The deposition takes place at 300 degrees Celsius. This can be of importance for some applications, but it gives a less dense film compared to LPCVD nitride, and the stoichiometry is on the following form: Si<sub>x</sub>N<sub>y</sub>O<sub>z</sub>H<sub>v</sub>. The step coverage and the thickness uniformity of the film are not as good as for the LPCVD nitride. In one of our PECVD systems (PECVD3) we allow small amounts of metal on the wafers entering the system; this is not allowed in the LPCVD furnace and in the clean PECVD (PECVD1). We also have a PECVD for deposition on III-V materials (PECVD2). | ||
*[[/Deposition of Silicon Nitride using PECVD|Deposition of Silicon Nitride using PECVD]] - ''or oxynitride'' | *[[/Deposition of Silicon Nitride using PECVD|Deposition of Silicon Nitride using PECVD]] - ''or oxynitride'' | ||
Latest revision as of 10:12, 11 May 2023
Feedback to this page: click here
Unless otherwise stated, this page is written by DTU Nanolab internal
Deposition of silicon nitride
Deposition of silicon nitride can be done by either LPCVD (Low Pressure Chemical Vapor Deposition) or PECVD (Plasma Enhanced Chemical Vapor Deposition). Stoichiometric nitride or silicon rich (low stress) LPCVD nitride is deposited on a batch of wafers in a LPCVD nitride furnace. PECVD nitride (or oxynitride) is deposited on a few samples at a time in a PECVD system. LPCVD nitride has a good step coverage and a very good uniformity. Using PECVD it is possible to deposit a much lower temperature and a thicker layer of nitride on different types of samples, but the nitride does not cover sidewalls very well.
It is also possible to deposit silicon nitride and oxynitride by reactive sputtering.
- Deposition of stoichiometric nitride using the 4" LPCVD nitride furnace
- Deposition of silicon rich (low stress) nitride using the 6" LPCVD nitride furnace
- Nitride deposition using PECVD (or oxynitride)
Comparison of LPCVD, PECVD, and sputter systems for silicon nitride deposition
LPCVD | PECVD | Sputter-System Metal-Nitride(PC3) and Sputter-System Metal-Oxide(PC1) | Lesker sputter system | |
---|---|---|---|---|
Generel description |
|
|
|
*Reactive sputtering |
Stoichiometry |
|
Silicon nitride can be doped with boron or phosphorus |
Tunable composition |
|
Film thickness |
Thicker nitride layers can be deposited over more runs (maximum two) |
|
|
|
Process temperature |
|
|
|
|
Step coverage |
|
|
|
|
Film quality |
|
|
|
|
KOH etch rate (80 oC) |
|
|
|
|
BHF etch rate |
|
|
|
|
Batch size |
|
Depending on what PECVD you use |
|
|
Allowed materials |
Processed wafers have to be RCA cleaned |
|
|
|