This page presents the results of TiN deposition using reactive sputtering by Lesker sputter tool. The source is Ti, and the reactive gas is N2. The fabrication and characterization were conducted in 2019 by Evgeniy Shkondin, DTU Nanolab. The prepared samples were investigated by X-ray Photoelectron Spectroscopy (XPS) and Spectroscopic Ellipsometry. Several parameters influences the quality of the films. The analysis included variations of power, pressure, substrate temperature and N2/Ar ratio.


In short, the key to prepare high quality, stochiometric, conducting TiN layers is to apply the following deposition parameters:


  • Before TiN deposition on the working wafer, always do pre-sputtering of Ti without N2 for around 2-3 min with the same power and pressure as desired for TiN.
    This will clean the target and decrease the level of moisture in the chamber.


  • High power in the range 220W-250W
    Lesker sputter tool uses 2-inch targets. For Ti source, the highest allowed power is 250W. Deposition rate increases by using high power and it lowers the incorporation of oxygen in the film.


  • Low pressure (1-2 mTorr)
    Lowering the pressure improves stochiometry and lowers the oxygen content.


  • High substrate temperature (400°C)
    Generally, the substrate temperature affects the density.


  • Work with N2 concentration in the range 20-50%
    The higher the nitrogen concentration the lower the deposition rate, and it will lead to problems with respect to oxygen contamination.


The investigation is based on two powers - 110W and 220W in the pressure range between 1 to 14 mTorr. The substrate temperature was kept at 400°C with N2/Ar ratio 20/80%.

Spectroscopic Ellipsometry

The spectroscopic ellipsometry measurements were conducted by using VASE Ellipsometer. The purpose of the investigation is to see how the change in deposition power and pressure affects the shape of the dielectric function. Other parameters - such as layer thickness were also extracted.

Drude-Lorentz model

Drude-Lorentz is commonly used to fit TiN complex dielectric function.


where: is a high-frequency dielectric constant.

The Drude term can be written as follow:


where: - dielectric permittivity of vacuum, - Planck constant, - resistivity, - scattering time.


Lorentz oscillator term is given by:


where: - number of oscillator, - Amplitude, - Broadening of each oscillator, - Center energy of the Lorentz oscillator.



Dielectric function analysis

High Power. Deposition time: 20min. Substrate temperature - 400°C Drude term Lorentz oscillator - 1 Lorentz oscillator - 2 Lorentz oscillator - 3
Power (W) Pressure (mTorr) Thickness (nm) (Ohm cm) (fs) (eV) (eV) (eV) (eV) (eV) (eV)
220 1 87.01 3.489 7.5618·10-5 1.008 192.557054 0.0213 6.321 9.689831 2.7132 5.604 - - -
220 2 66.13 2.609 2.017·10-4 1.141 2.083940 0.8848 3.492 8.125820 3.2412 5.944 15.781023 0.9923 1.053
220 4 66.40 1.934 6.6567·10-4 1.041 2.439534 1.3777 3.724 4.677488 4.0837 6.160 12.110575 0.9458 0.959
220 6 75.11 1.347 2.587·10-3 0.655 2.303432 1.7123 3.942 1.934678 5.4051 6.420 7.712139 0.9659 0.883
220 8 81.94 1.271 4.273·10-3 0.242 2.038004 1.7074 4.062 1.614453 5.6564 6.677 5.212949 0.8602 0.895
220 10 82.59 1.138 5.257·10-3 0.323 1.672949 1.6265 4.186 1.433617 7.9416 7.058 4.294563 0.8546 0.902
220 12 82.40 1.090 5.807·10-3 0.443 1.450316 1.5414 4.262 1.368362 9.1405 7.128 3.787770 0.8471 0.906
220 14 81.88 1.089 5.838·10-3 0.468 1.415215 1.5370 4.266 1.349390 9.2650 7.074 3.579245 0.8420 0.909
Low Power. Deposition time: 40min. Substrate temperature - 400°C Drude term Lorentz oscillator - 1 Lorentz oscillator - 2 Lorentz oscillator - 3
Power (W) Pressure (mTorr) Thickness (nm) (Ohm cm) (fs) (eV) (eV) (eV) (eV) (eV) (eV)
110 2 37.28 1.951 3.4619·10-4 0.719 2.294032 2.7712 4.298 8.807626 4.6007 7.311 14.494131 1.0222 1.025
110 4 32.42 2.024 9.724·10-4 0.890 5.185267 3.5747 4.958 7.900142 2.2325 7.115 12.284271 0.8444 1.012
110 6 34.12 1.907 2.109·10-3 1.119 3.946173 3.4395 4.953 4.368733 1.9486 7.189 7.063107 0.8046 0.983
110 8 35.58 1.694 2.661·10-3 1.292 2.990718 3.3861 4.928 3.091825 2.0160 7.163 4.843337 0.7813 0.980
110 10 37.02 1.526 2.741·10-3 1.592 2.521075 3.5788 4.959 2.664635 2.1239 7.295 3.751751 0.7497 0.975



Dielectric function can be rearranged in order to separate real and complex parts: . Here, is a real part of the permittivity, and is imaginary part describing optical losses.


Process power and pressure is extremely important values since the slightest deviation will change the TiN optical performance. The clear metallic behavior is observed at lowest pressure and the highest power. Decreasing the power and/or increasing the process pressure will change the metallic state into oxynitride and oxide phase response.

DC power 220W

At this power, the metallic response (negative values of ) can be observed in the pressure range below 3mTorr, although only 1 and 2 mTorr can be used in plasmonic applications. A small variation in thickness should not severely affect the shape of permittivity function.

DC power 110W

At low power, the metallic response (negative values of ) can be observed in the pressure range below 2mTorr, although it never become strongly negative. The deposition rate is 4 times lower compared to 220W, which unavoidably leads to oxygen incorporation in the film. A small variation in thickness should not severely affect the shape of permittivity function.

XPS analysis

XPS measurements of all samples has been performed using XPS K-Alpha equipment. The purpose of the investigation is to see how the change in deposition power and pressure affects the stochiometry and elemental peak shape.

High resolution scans of individual elements

The prepared TiN films were Ar+ sputtered-cleaned prior to measurements. The Ti 2p scans are the most informative. They clearly show that the lower the process pressure the more present Ti-N bounding in the deposited film. This tendency presents most clearly in the highest chosen power 220W. The conclusion support the result form the ellipsometry measurements - the metallic TiN films grows at low pressure and high power.

DC power 220W

DC power 110W

Stochiometry and N2/Ti ratio

XPS Avantage software package has been used to extract information about chemical composition and presence of the deposited TiN films. the presence of C is not properly understood. This is not an air-born adventitious carbon, since the deposited films, were Ar+ sputtered-cleaned. The contamination could come from the Ti target source, incorporation of C from the air into the film structure or background chamber contamination.

Power (W) Pressure (mTorr) Ti (At. %) N (At. %) O (At. %) C (At. %)
220 14 35.20 27.26 33.34 4.20
220 12 35.93 27.71 34.00 2.36
220 10 36.02 27.68 33.34 2.96
220 8 36.23 27.74 32.93 3.10
220 6 35.74 28.49 32.08 3.69
220 4 36.19 29.78 30.05 3.98
220 2 37.12 32.33 26.08 4.47
220 1 42.51 39.27 16.75 1.48
110 10 35.31 26.76 33.84 4.08
110 8 35.86 27.01 32.91 4.22
110 6 35.64 27.24 32.03 5.09
110 4 34.74 27.35 30.34 7.56
110 2 37.18 30.26 27.08 5.48


Ideally, the N2/Ti ratio should be equal to 1. However, the presence of oxynitride/oxide phase lowers this value. In general, the stochiometry improves by raising the power and lowering the process pressure.

Effect of substrate temperature

Preparation of high-quality metallic TiN thin films require high substrate temperature. This method excludes the possibility to deposit TiN on temperature sensitive materials - like photoresist. Normally, the substrate temperature affects the density of the deposited film. Only room temperatur vs. 400oC has been analyzed here. The conclusion is clear - high temperature is the key to get the good plasmonic films.

High Power. Deposition time: 10min Drude term Lorentz oscillator - 1 Lorentz oscillator - 2 Lorentz oscillator - 3
Temperature (oC) Power (W) Pressure (mTorr) Thickness (nm) (Ohm cm) (fs) (eV) (eV) (eV) (eV) (eV) (eV)

20

220 2 41.06 2.574 6.5701·10-4 0.815 5.851313 6.8806 6.711 14.513401 1.0293 1.038 - - -

400

220 2 46.09 2.692 2.1618·10-4 0.697 1.087128 1.3685 3.824 8.301574 3.5998 6.291 10.301534 1.0371 1.104



Effect of N2/Ar ratio

High Power. Deposition time: 20min Drude term Lorentz oscillator - 1 Lorentz oscillator - 2 Lorentz oscillator - 3
N2 (flow (%)) Power (W) Pressure (mTorr) Thickness (nm) (Ohm cm) (fs) (eV) (eV) (eV) (eV) (eV) (eV)

20

220 1 87.01 3.489 7.5618·10-5 1.008 192.557054 0.0213 6.321 9.689831 2.7132 5.604 - - -