Specific Process Knowledge/Lithography/LiftOff: Difference between revisions
Appearance
| (4 intermediate revisions by 2 users not shown) | |||
| Line 34: | Line 34: | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
NMP (Remover 1165) | Lift-off bath with NMP (Remover 1165) | ||
Rinse bath with diluted IPA | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
User defined | User defined | ||
| Line 133: | Line 135: | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*NMP (Remover 1165) | *NMP (Remover 1165) | ||
*Rinse in IPA | *Rinse in diluted IPA | ||
|- | |- | ||
!style="background:silver; color:black" valign="center" rowspan="2"|Process parameters | !style="background:silver; color:black" valign="center" rowspan="2"|Process parameters | ||
| Line 201: | Line 203: | ||
'''Problem:''' Mathias experienced the delamination of TiAu after the lift-off process, see the image. | '''Problem:''' Mathias experienced the delamination of TiAu after the lift-off process, see the image. | ||
'''Solution:''' Adding a descum step (70 ml/min O2, 70 ml/min N2, 150W, 5 min) right before metal depositions. | '''Solution:''' Adding a descum step (70 ml/min O2, 70 ml/min N2, 150W, 5 min (Plasma Asher 1)) right before metal depositions. | ||
[[File:Delamination of TiAu.jpg|thumb]] | [[File:Delamination of TiAu.jpg|thumb]] | ||
| Line 213: | Line 215: | ||
3.) Development of nLOF | 3.) Development of nLOF | ||
'''4.) 5 min descum (70 ml/min O2, 70 ml/min N2, 150W, 5 min in Plasma Asher 1) was done right before TiAu deposition''' | |||
5.) 10 nm Ti depositing with 2 A/s by Temescal | 5.) 10 nm Ti depositing with 2 A/s by Temescal | ||
| Line 221: | Line 223: | ||
7.) Lift-off (approx. 45 min) | 7.) Lift-off (approx. 45 min) | ||
By adding step 4.) 5 min Descum, the problem with the delamination of metals was solved. | |||