<?xml version="1.0"?>
<feed xmlns="http://www.w3.org/2005/Atom" xml:lang="en">
	<id>https://labadviser.nanolab.dtu.dk//index.php?action=history&amp;feed=atom&amp;title=Specific_Process_Knowledge%2FPolymer_Processing%2FPDMS_Post-processing</id>
	<title>Specific Process Knowledge/Polymer Processing/PDMS Post-processing - Revision history</title>
	<link rel="self" type="application/atom+xml" href="https://labadviser.nanolab.dtu.dk//index.php?action=history&amp;feed=atom&amp;title=Specific_Process_Knowledge%2FPolymer_Processing%2FPDMS_Post-processing"/>
	<link rel="alternate" type="text/html" href="https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Polymer_Processing/PDMS_Post-processing&amp;action=history"/>
	<updated>2026-11-06T02:44:20Z</updated>
	<subtitle>Revision history for this page on the wiki</subtitle>
	<generator>MediaWiki 1.43.3</generator>
	<entry>
		<id>https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Polymer_Processing/PDMS_Post-processing&amp;diff=57156&amp;oldid=prev</id>
		<title>Cchvi at 10:21, 5 November 2026</title>
		<link rel="alternate" type="text/html" href="https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Polymer_Processing/PDMS_Post-processing&amp;diff=57156&amp;oldid=prev"/>
		<updated>2026-11-05T10:21:14Z</updated>

		<summary type="html">&lt;p&gt;&lt;/p&gt;
&lt;table style=&quot;background-color: #fff; color: #202122;&quot; data-mw=&quot;interface&quot;&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;tr class=&quot;diff-title&quot; lang=&quot;en&quot;&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;← Older revision&lt;/td&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;Revision as of 11:21, 5 November 2026&lt;/td&gt;
				&lt;/tr&gt;&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l1&quot;&gt;Line 1:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 1:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The fabrication of microfluidic devices requires further processing of PDMS, including cutting, creating through-holes,  &lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The fabrication of &lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;PDMS &lt;/ins&gt;microfluidic devices requires further processing of PDMS &lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;once it has been casted and cured&lt;/ins&gt;, including cutting, creating through-holes,  &lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;bonding to other parts, and surface functionalization.&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;bonding to other parts, and surface functionalization. &lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;Details on PDMS casting are described in [https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Polymer_Processing/PDMS_Casting PDMS Casting]&lt;/ins&gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;[[File:Processing of PDMS .png|1000px|frame|center|Fabrication of microfluidic device by casting of PDMS on SU-8/silicon mould, folowed by punching of through holes, and glass, vial bonding]]&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;[[File:Processing of PDMS .png|1000px|frame|center|Fabrication of microfluidic device by casting of PDMS on SU-8/silicon mould, folowed by punching of through holes, and glass, vial bonding]]&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt; &lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;[[File:PDMS lab process.jpg|center|frame|Process for PDMS in DTU Nanolab, work done by Claudia Chaves Villarreal cchvi@dtu.dk]]&lt;/ins&gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;==Cutting of PDMS==&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;==Cutting of PDMS==&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;/table&gt;</summary>
		<author><name>Cchvi</name></author>
	</entry>
	<entry>
		<id>https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Polymer_Processing/PDMS_Post-processing&amp;diff=57153&amp;oldid=prev</id>
		<title>Cchvi: Created page with &quot; The fabrication of microfluidic devices requires further processing of PDMS, including cutting, creating through-holes,  bonding to other parts, and surface functionalization. Fabrication of microfluidic device by casting of PDMS on SU-8/silicon mould, folowed by punching of through holes, and glass, vial bonding  ==Cutting of PDMS==  Cutting of PDMS is a common step in the fabrication of PDMS microfluidics  to create...&quot;</title>
		<link rel="alternate" type="text/html" href="https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Polymer_Processing/PDMS_Post-processing&amp;diff=57153&amp;oldid=prev"/>
		<updated>2026-11-05T10:11:10Z</updated>

		<summary type="html">&lt;p&gt;Created page with &amp;quot; The fabrication of microfluidic devices requires further processing of PDMS, including cutting, creating through-holes,  bonding to other parts, and surface functionalization. &lt;a href=&quot;/index.php?title=File:Processing_of_PDMS_.png&quot; title=&quot;File:Processing of PDMS .png&quot;&gt;1000px|frame|center|Fabrication of microfluidic device by casting of PDMS on SU-8/silicon mould, folowed by punching of through holes, and glass, vial bonding&lt;/a&gt;  ==Cutting of PDMS==  Cutting of PDMS is a common step in the fabrication of PDMS microfluidics  to create...&amp;quot;&lt;/p&gt;
&lt;p&gt;&lt;b&gt;New page&lt;/b&gt;&lt;/p&gt;&lt;div&gt;&lt;br /&gt;
The fabrication of microfluidic devices requires further processing of PDMS, including cutting, creating through-holes, &lt;br /&gt;
bonding to other parts, and surface functionalization.&lt;br /&gt;
[[File:Processing of PDMS .png|1000px|frame|center|Fabrication of microfluidic device by casting of PDMS on SU-8/silicon mould, folowed by punching of through holes, and glass, vial bonding]]&lt;br /&gt;
&lt;br /&gt;
==Cutting of PDMS==&lt;br /&gt;
&lt;br /&gt;
Cutting of PDMS is a common step in the fabrication of PDMS microfluidics  to create access ports, also known as througholes, or for separating the individual devices from a microfluidic PDMS wafer. The PDMS lab thrives on providing the optimal tools and processes for the users. Common tools that are provided in the lab for manual cutting are tweezers, blades, cutting mats, light screen and press. &lt;br /&gt;
&lt;br /&gt;
[[File:PDMS through-hole methods.jpg|999px|right|frame|link=|Scanning Electron Microscopy (SEM) micrographs for comparison of methods to fabricate through-holes in PDMS, work done by Claudia Chaves Villarreal cchvi@dtu.dk]]&lt;br /&gt;
&lt;br /&gt;
Alternative methods for high-throughput fabrication are under investigation at Nanolab to meet the demands of the industry and large interdisciplinary projects. The cutting methods being researched include the development of wafer-size punching, laser ablation,  mechanical and air/water jet machining.&lt;br /&gt;
&lt;br /&gt;
&lt;br /&gt;
&amp;#039;&amp;#039;&amp;#039;Punching&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
&lt;br /&gt;
[[File:Manual puncher.jpg|thumb|Example of a 20 mm commercial puncher used to cut individual chips out of a PDMS microfluidic wafer]] &lt;br /&gt;
&lt;br /&gt;
The access ports of microfludic devices, also known as through-holes, can be created using manual punchers commercially available for biopsy or general use. Always punch the devices on top of the green cutting board to extend the lifetime of the puncher blade and to avoid marking the table. Solvents like ethanol, isopropanol and acetone can be used as lubricants to facilitate the cutting and result in a cleaner surface. All solvents must be always used inside the fume hood. The resulting punched holes in PDMS tend to be slightly smaller than the puncher diameter, smo, the final dimensions of the holes must be confirmed with metrology methods.&lt;br /&gt;
&lt;br /&gt;
&amp;#039;&amp;#039;&amp;#039;Laser ablation&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
&lt;br /&gt;
The ultra short pulsed laser (pisecond to femtosecond) can be used as a &amp;quot;cold machining&amp;quot; approach to cut transparent dielectrics like PDMS. At DTU Nanolab, the [https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Back-end_processing/Laser_Micromachining_Tool Laser Micromachining Tool] can be used for processing PDMS. &lt;br /&gt;
&lt;br /&gt;
&amp;#039;&amp;#039;&amp;#039;Machining/milling&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
&lt;br /&gt;
&amp;#039;&amp;#039;&amp;#039;Air/water jet machining&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
&lt;br /&gt;
==3D printing of PDMS==&lt;br /&gt;
&lt;br /&gt;
Soft-litography micromolding and cutting protocols pose limitations for complex designs, require long processing times, and are labour intensive. 3D printing of PDMS provides the automation and versatility features to meet the demands for future technologies. The 3D printing of PDMS is currently under development at Nanolab.&lt;br /&gt;
&lt;br /&gt;
==PDMS cleaning==&lt;br /&gt;
[[File:20260804 115934.jpg|thumb|Ultrasonic bath for cleaning the PDMS devices]]&lt;br /&gt;
&lt;br /&gt;
The processing of PDMS may contaminate its surface yielding it inadequate for its final application, or affecting its surface for further bonding. Cutting with sharp tools like puncher and milling may leave reasidues of PDMS particles and lubricants. Laser ablation may leave silicone powder, carbon, ashes, and further by-products of the thermal decomposition. The manipulation may also contaminate it with grease or particles from the environment.&lt;br /&gt;
&lt;br /&gt;
==PDMS surface modification==&lt;br /&gt;
&lt;br /&gt;
Different physical and chemical treatments can modify the wettability, refractive index, and light propagation of PDMS, due to both chemical bond rearrangements and changes in surface roughness. &lt;br /&gt;
&lt;br /&gt;
&amp;#039;&amp;#039;&amp;#039;Chemical treatment&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
&lt;br /&gt;
&amp;#039;&amp;#039;&amp;#039;Laser treatment&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
&lt;br /&gt;
==Bonding of PDMS==&lt;br /&gt;
&lt;br /&gt;
In many applications, including microfluidics, it is necessary to bond the PDMS microfluidic chips to glass, PMMA, other PDMS parts and more. In this section we describe the methods so far used for creating stron, long-lasting bonds.&lt;br /&gt;
&lt;br /&gt;
&lt;br /&gt;
&amp;#039;&amp;#039;&amp;#039;Bonding of PDMS to glass and other PDMS parts&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
&lt;br /&gt;
[[File:Plasma Treatment.jpg|thumb|(left) PDMS microfluidic chips and glass placed inside plasma system. (right) Plasma generated inside the system to activate PDMS and glass surfaces  ]]&lt;br /&gt;
[[File:Bonding of PDMS and glass for fabrication of microfluidic device.jpg|thumb|Bonding of oxygen plasma-treated PDMS and glass for fabrication of microfluidic device]]&lt;br /&gt;
[[File:Press for bonding PDMS microfluidics.jpg|thumb|Press used to improve the bonding of PDMS and glass in a microfluidic device]]&lt;br /&gt;
[[File:Standard plasma treatment condition to bond glass and PDMS.jpg|thumb|Standard conditions of the plasma treatment to bond glass and PDMS]]&lt;br /&gt;
Oxygen plasma treatment of PDMS and glass surfaces can be used for bonding. The plasma induces activation of Si-O-H groups in the surface of glass and PDMS, which induces a strong bond when the surfaces are shortly brought into contact. The plasma equipment requires to login in LabManager, after proper training by Nanolab staff. &lt;br /&gt;
&lt;br /&gt;
The modified surface will fastly recover its hydrophobic structure. Therefore, the treated surfaces must be brought into contact immediately after the plasma had been applied.  &lt;br /&gt;
&lt;br /&gt;
A press is available in the lab  to hold parts under pressure after brought into contact  to reinforce the bonding.&lt;br /&gt;
&lt;br /&gt;
The oxygen plasma treatment to apply must be optimized for the specific surfaces to be bonded. If the exposure is too short, not enough Si-OH sites might be created for good bonding. If the exposure is too long, too many Si-OH and roughness might result in a non-sticking silica layer. &lt;br /&gt;
&lt;br /&gt;
The standard conditions for bonding PDMS and glass in the system at the PDMS lab at DTU Nanolab have been found to be:&lt;br /&gt;
&lt;br /&gt;
*Pressure: 0.35 mTorr&lt;br /&gt;
&lt;br /&gt;
*Oxygen flow: 100% (5-6sccm)&lt;br /&gt;
&lt;br /&gt;
*Power: 100%&lt;br /&gt;
&lt;br /&gt;
*Time: 30 s&lt;br /&gt;
&lt;br /&gt;
The plasma treatment above described does not induce any permanent chemical modification to the glass or PDMS, as demonstrated by XPS analysis.   &lt;br /&gt;
&lt;br /&gt;
[[File:Contact Angle Plasma Tretament vs Time.jpg|1000px|thumb|center|Pictures of contact angle for water drop on PDMS and borosilicate glass after plasma treatment in the PDMS lab at DTU for different time, work done by Claudia Chaves Villarreal cchvi@dtu.dk]]&lt;br /&gt;
[[File:Contact angle vs plasma time.png|1000px|thumb|center|Graphs of contact angle for water on PDMS and borosilicate glass vs oxygen plasma treatment time, work done by Claudia Chaves Villarreal cchvi@dtu.dk]]&lt;br /&gt;
[[File:PMMA PDMS bonding.jpg|thumb|Bonding of cured PDMS and PMMA parts using uncured PDMS as glue]]&lt;br /&gt;
[[File:PMMA plasma treatment.png|thumb|Surface activation of PMMA with oxygen plasma for bonding with PDMS]]&lt;br /&gt;
&lt;br /&gt;
&amp;#039;&amp;#039;&amp;#039;Bonding of PDMS to PMMA&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
&lt;br /&gt;
PDMS can be bonded to other polymers, like PMMA, for interfacing the microstructured patterns with tubes, vials and other macroscopic parts. The Sylgard 184 elastomer kit can be used as a &amp;quot;glue&amp;quot; between PMMA and cured PDMS, provided that an extended curing time of 24 hours at 70°C is applied to create a robust bond between the two surfaces. Roughening the PMMA surface beforehand may result in stronger adhesion.&lt;br /&gt;
&lt;br /&gt;
The standard conditions for PMMA treating before confing to PDMS in the system at the PDMS lab at DTU Nanolab have been found to be:&lt;br /&gt;
&lt;br /&gt;
*Pressure: 0.35 mTorr&lt;br /&gt;
&lt;br /&gt;
*Oxygen flow: 100% (5-6sccm)&lt;br /&gt;
&lt;br /&gt;
*Power: 100%&lt;br /&gt;
&lt;br /&gt;
*Time: 120 s&lt;br /&gt;
&lt;br /&gt;
==Contact and access==&lt;br /&gt;
&lt;br /&gt;
For further information contact [https://www.nanolab.dtu.dk/polyfablab PolyFablLab]&lt;/div&gt;</summary>